Method for reducing residual stress of 7xxx series aluminum alloy thick plate
Through a combination of solution treatment, cryogenic rolling and aging treatment, the problem of quenching residual stress and corrosion resistance of 7xxx series aluminum alloy thick plates has been solved, the residual stress has been significantly reduced and the overall performance of the material has been improved.
Patent Information
- Application Number
- CN202411038110.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-10-08
AI Technical Summary
The huge quenching residual stress introduced during the solution quenching process of 7xxx series aluminum alloy thick plates has a negative impact on subsequent processing and forming, and affects the stress corrosion resistance of the material.
After solid solution treatment, it is quickly cooled to room temperature, and then multiple passes of cryogenic rolling are performed until the total reduction rate reaches 20% to 30%, followed by aging treatment. The temperature field and solution quenching process during the cryogenic rolling process On the contrary, it offsets the residual stress and weakens the quenching residual stress through the stress field introduced by plastic deformation in the cryogenic environment, promotes the diffusion of Cu elements and the formation of precipitated phases, and improves the corrosion resistance of the material.
The quenching residual stress is significantly reduced by 70% to 80%, and the comprehensive corrosion resistance of the material is improved through the aging process, resulting in a 7xxx series aluminum alloy plate with excellent mechanical properties.
Smart Images

Figure CN118745562A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal material deformation and heat treatment, and in particular relates to a method for reducing residual stress of a 7xxx series aluminum alloy thick plate. Background Art
[0002] 7xxx series aluminum alloys have high specific strength, specific stiffness, and excellent comprehensive service performance. They can well meet the needs of lightweight industrial production and are widely used in aerospace and transportation. Among them, 7xxx series aluminum alloy thick plates are often used in aerospace and large transportation equipment. A very important problem in the production and processing process is that huge quenching residual stress will be introduced during the solid solution quenching process, which will have an adverse effect on its subsequent processing and forming. It is of great significance to study how to weaken the quenching residual stress of 7xxx series aluminum alloy thick plates.
[0003] In the traditional aluminum alloy processing, in order to obtain a more complete precipitation strengthening effect and improve the processing performance of the material, solution quenching treatment is often necessary. Considering the quenching sensitivity of the material, the quenching process is required to be completed in a very short time to ensure the supersaturated solid solution state of the material, so as to obtain more strengthening precipitation phases in the subsequent aging process. However, the increase in quenching rate will also bring greater residual stress, which will have a considerable damage to the material's stress corrosion resistance and have a significant impact on the subsequent component formability and dimensional stability. Summary of the invention
[0004] In order to overcome the above-mentioned shortcomings of the prior art, the object of the present invention is to provide a method for reducing the residual stress of 7xxx series aluminum alloy thick plates, so as to weaken the quenching residual stress of 7xxx series aluminum alloy plates and improve their corrosion resistance.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for reducing residual stress in a 7xxx series aluminum alloy thick plate comprises the following steps:
[0007] The first step is to perform a solution treatment on the 7xxx aluminum alloy plate at a solution treatment temperature of 748K±3K for 1h to 2h;
[0008] The second step is to take out the solution treated plate and quickly place it in room temperature water for quenching and cool it to room temperature;
[0009] The third step is to perform multiple passes of deep cold rolling on the 7xxx aluminum alloy sheet after cooling in the second step until the total reduction rate reaches 20% to 30%, wherein the deep cold rolling means that the temperature of the sheet during the rolling process is 77K to 97K;
[0010] The fourth step is to perform aging treatment on the plate obtained by multiple deep cold rolling, and the aging system is 394K±3K, 6 to 8h, and then 450K±3K, 3 to 5h.
[0011] In one embodiment, the 7xxx aluminum alloy sheet is a 7050 aluminum alloy sheet, a 7075 aluminum alloy sheet, or the like.
[0012] In one embodiment, the 7xxx aluminum alloy plate has a thickness of 5 mm to 35 mm.
[0013] In one embodiment, the steps of the multi-pass deep cold rolling are as follows:
[0014] Step 1, placing the 7xxx aluminum alloy plate in a deep freezer for cooling, so that its temperature is uniformly reduced to 77K to 97K;
[0015] Step 2, taking out the cooled plate for rolling, with a rolling speed of 3.5-5.5 m / min and a pass reduction rate of 4%-6%;
[0016] Step 3, repeat steps 1 and 2 until the total reduction rate meets the requirements.
[0017] The main principle of the present invention is that during the deep cold rolling process, the temperature field distribution of the 7xxx aluminum alloy material is opposite to the temperature field distribution during the solution quenching process, thereby generating an opposite stress field, which can offset a portion of the quenching residual stress and reduce the residual stress generated during the solution quenching process of the 7xxx aluminum alloy material. In addition, the stress field introduced by the lattice distortion during the plastic deformation process under the deep cold environment also weakens the quenching residual stress to a certain extent. The combined effect of the two factors significantly reduces the quenching residual stress of the aluminum alloy thick plate.
[0018] At the same time, the deep cold rolling process retains more dislocations in the material by suppressing the recovery behavior, providing more energy and nucleation sites for the subsequent aging process, promoting the diffusion of Cu elements and the formation and growth of precipitates. Larger and more dispersed precipitates at the grain boundaries can hinder the development of intergranular corrosion. The increase in the Cu content at the grain boundaries is also conducive to reducing the potential difference between the precipitates and the matrix, thereby reducing the corrosion rate. This improves the comprehensive corrosion resistance of the material.
[0019] Experiments have shown that the 7xxx series aluminum alloy plate prepared by the method of the present invention has lower residual stress, and the residual stress of the plate pre-deformed by deep cold rolling is reduced by 70% to 80% compared with the solution quenching state, and combined with an appropriate aging system, it can obtain better corrosion resistance than the traditional process. Due to its low processing cost and simple process flow, it has broad application prospects in the industrial processing of medium and thick plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 It is a flow chart of the method of the present invention.
[0021] Figure 2 It is a schematic diagram of the strain response of the solid solution state and rolled state plates of the product obtained in Example 1 of the present invention when cutting.
[0022] Figure 3 This is the polarization curve of the plate after deep cold rolling, room temperature rolling and aging treatment in Example 2 of the present invention.
[0023] Figure 4 These are the impedance curves of the deep cold rolled samples, room temperature rolled samples and aged samples in Example 2 of the present invention.
[0024] Figure 5 It is the Bode diagram of the deep cold rolled sample, the room temperature rolled sample and the aged sample in Example 2 of the present invention.
[0025] Figure 6 This is the intergranular corrosion morphology of the deep cold rolled and room temperature rolled samples after aging in Example 2 of the present invention. DETAILED DESCRIPTION
[0026] The embodiments of the present invention are described in detail below with reference to the accompanying drawings and examples.
[0027] The present invention is a method for reducing residual stress in 7xxx series aluminum alloy thick plates. Figure 1 As shown, it mainly includes the following steps:
[0028] Step 1: Use 7xxx aluminum alloy sheet with a thickness of 5mm to 35mm.
[0029] Step 2: Solution treatment of 7xxx aluminum alloy plate at a temperature of 748K±3K for 1 to 2h.
[0030] Step 3: Take out the solution treated plate and quickly place it in room temperature water for quenching and cool it to room temperature.
[0031] Step 4: Place the 7xxx aluminum alloy sheet at room temperature in a cryogenic box for cooling, and wait until its temperature is uniformly reduced to 77K to 97K. The cryogenic box here can be a box containing a cryogenic medium such as liquid nitrogen.
[0032] Step 5: Take out the cooled plate and immediately roll it at a speed of 3.5-5.5 m / min. The reduction rate per pass is 4%-6%.
[0033] Step 6: Repeat steps 4 and 5 until the total reduction rate reaches 20% to 30%. After multiple passes of deep cold pre-rolling, the residual stress can be significantly reduced while the strength is improved, thus achieving the reduction of residual stress of the material. Experiments have shown that the absolute value of residual stress of the plate after deep cold rolling is reduced by 70% to 80% compared with that of the solid solution plate. At the same time, due to the deformation strengthening of pre-rolling, the strength of the material is also improved to a certain extent.
[0034] Step 7: Aging treatment is performed on the plate, and the aging system is 6 to 8 hours at 394K±3K and 3 to 5 hours at 450K±3K. During the aging process, more dislocations introduced by the deep cold rolling process can promote precipitation behavior, thereby improving the comprehensive corrosion performance of the material and improving the corrosion resistance of the material.
[0035] Therefore, the present invention can effectively reduce the residual stress generated during the solid solution quenching process of the material through deep cold rolling combined with subsequent aging, and obtain 7xxx series aluminum alloy plates with both excellent mechanical properties and corrosion resistance.
[0036] Two specific embodiments of the present invention are as follows.
[0037] Example 1
[0038] Step 1: Use 7050 aluminum alloy sheet with a thickness of 30mm.
[0039] Step 2: Solution treatment of 7050 aluminum alloy plate, the solution treatment temperature is 748K, and the time is 2h.
[0040] Step 3: Quench the solution treated plate in water at room temperature and cool it to room temperature.
[0041] Step 4: Immerse the room temperature 7050 aluminum alloy sheet in a deep freezer for cooling, so that the temperature of the material is uniformly reduced to 77K.
[0042] Step 5: Roll the cooled plate at a rolling speed of 4 m / min and control the reduction rate of each pass at 4% to 6%.
[0043] Step 6: Repeat steps 4 and 5 until the total reduction rate reaches 20% and the product thickness is 24 mm. The strength of the prepared pre-rolled aluminum alloy sheet is 120 MPa higher than that before pre-rolling, reaching 520 MPa. The residual stress of the sheet after deep cold rolling is reduced by 83% through crack compliance method test analysis, indicating that this process can significantly reduce the quenching residual stress of the material and has good prospects in industrial application. Figure 2 The strain response of the crack back changes with the cutting depth during EDM cutting of solution and rolled plates. The results provide the original data for the analysis of the crack compliance method.
[0044] Step 7: Aging treatment is performed on the parts at 394K for 6 hours and then at 450K for 3 hours. The aging heat treatment process can further weaken the residual stress of the material and obtain excellent comprehensive mechanical properties suitable for industrial applications.
[0045] Example 2
[0046] Step 1: Use 7050 aluminum alloy sheet with a thickness of 6mm.
[0047] Step 2: Solution treatment of 7050 aluminum alloy plate, the solution treatment temperature is 748K, and the time is 2h.
[0048] Step 3: Quench the solution treated plate in water at room temperature and cool it to room temperature.
[0049] Step 4: Immerse the room temperature 7050 aluminum alloy sheet in a deep freezer for cooling, so that the temperature of the material is uniformly reduced to 77K.
[0050] Step 5: Roll the cooled plate at a rolling speed of 4 m / min. The pass reduction rate is controlled at 4% to 6%.
[0051] Step 6: Repeat Step 4 and Step 5 until the total reduction rate reaches 30% and the product thickness is 4.2 mm. The strength of the prepared pre-rolled aluminum alloy sheet is increased by 170 MPa compared with that before pre-rolling, reaching 570 MPa.
[0052] Step 7: Aging treatment of the parts, aging at 394K for 6 hours, and then aging at 450K for 3 hours. Electrochemical corrosion test and intergranular corrosion test were carried out on the aged samples to test the corrosion resistance of the materials. The results are as follows: Figures 3 to 6 As shown, Figure 3 The electrochemical polarization curves of the deep cold rolled sample, the room temperature rolled sample and the two samples after aging were compared. It can be seen that in the rolled state, the difference between the two samples is not large. After aging, the deep cold rolled sample has a higher corrosion potential and a lower corrosion current density. Figure 4 and Figure 5 Comparing the impedance curves of the deep cold rolled sample, the room temperature rolled sample and the two samples after aging, it can be clearly seen that the deep cold rolled sample has a higher impedance; Figure 6 The intergranular corrosion morphology of deep cold rolled samples and room temperature rolled samples after aging was compared. According to statistics, after aging, the maximum depth of intergranular corrosion of deep cold rolled samples was reduced by 10% and the average depth of intergranular corrosion was reduced by 8% compared with room temperature rolled samples. The above results all show that deep cold rolling combined with subsequent aging can effectively improve the corrosion resistance of the material.
Claims
1. A method for reducing residual stress in a 7xxx series aluminum alloy thick plate, characterized in that: The steps include: The first step is to perform a solution treatment on the 7xxx aluminum alloy plate at a temperature of 748K±3K for 1 to 2 hours; The second step is to take out the solution treated plate and quickly place it in room temperature water for quenching and cool it to room temperature; The third step is to perform multiple passes of deep cold rolling on the 7xxx aluminum alloy sheet after cooling in the second step until the total reduction rate reaches 20% to 30%, wherein the deep cold rolling means that the temperature of the sheet during the rolling process is 77K to 97K; The fourth step is to perform aging treatment on the plate obtained by multiple deep cold rolling, and the aging system is 394K±3K, 6 to 8h, and then 450K±3K, 3 to 5h.
2. The method for reducing residual stress in a 7xxx series aluminum alloy thick plate according to claim 1, characterized in that: The 7xxx aluminum alloy sheet is a 7050 aluminum alloy sheet or a 7075 aluminum alloy sheet.
3. The method for reducing residual stress in 7xxx series aluminum alloy thick plate according to claim 1 or 2, characterized in that: The thickness of the 7xxx aluminum alloy plate is 5 mm to 35 mm.
4. The method for reducing residual stress in a 7xxx series aluminum alloy thick plate according to claim 1, characterized in that: The steps of the multi-pass deep cold rolling are as follows: Step 1, placing the 7xxx aluminum alloy plate in a deep freezer for cooling, so that its temperature is uniformly reduced to 77K to 97K; Step 2, taking out the cooled plate for rolling, with a rolling speed of 3.5-5.5 m / min and a pass reduction rate of 4%-6%; Step 3, repeat steps 1 and 2 until the total reduction rate meets the requirements.
Citation Information
Patent Citations
Rolled aluminum alloy copious cooling treatment method
CN108203795A
Method for eliminating residual stress of aluminum alloy die forging piece
CN109112449A
Cryorolling and aging treatment process for high-strength Al-Zn-Mg alloy
CN110964957A
Method for producing 7000 series aluminum alloy member excellent in stress corrosion crack resistance
JP2019011511A
Cited By
Treatment method of 2-series aluminum alloy plate
CN119824344A