Preparation method and application of graphene / nano-copper composite conductive film

The preparation method of graphene/nano-copper composite conductive film solves the problems of high cost and difficult manufacturing of traditional electrochemical sensors, improves nitrate detection performance, and achieves efficient nitrate detection, which is suitable for agriculture and ecological environment protection needs. .

CN118745587APending Publication Date: 2024-10-08SANYA HANENE GRAPHENE TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410730959.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Traditional electrochemical sensors have limited the development of agriculture and ecological environment due to their high cost and difficulty in manufacturing, especially inefficiency in nitrate detection.

Method used

Using the preparation method of graphene/nano-copper composite conductive film, the graphene film is treated by carbonization, annealing and rolling, and copper nanoparticles are deposited by electrochemical deposition, combined with sandpaper polishing surface treatment to form a ravine structure to increase the surface area and copper The loading capacity of nanoparticles is suitable for electrochemical sensor nitrate detection.

Benefits of technology

It achieves the high conductivity and flexibility of the graphene film, while improving the binding force and stability of copper nanoparticles, enhancing the detection performance of nitrate radicals, simplifying the production process, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745587A_ABST
    Figure CN118745587A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a graphene / nano-copper composite conductive film, and relates to the technical field of graphene composite materials. According to the method, the graphene film is prepared firstly, then the copper nanoparticles are deposited on the graphene film in an electrochemical deposition mode, the deposition process of the copper nanoparticles can be accurately regulated and controlled, the binding force between the copper nanoparticles and the graphene film is effectively increased, and it is ensured that the copper nanoparticles are stably attached to the surface of the graphene film; the surface treatment mode of abrasive paper polishing is adopted, so that the surface area of the graphene film is remarkably increased, the loading number of copper nanoparticles is increased, and the active sites of electrochemical nitrate sensing are improved. Through the mode, the flexible graphene / nano-copper composite conductive film with high conductivity is prepared, and the composite conductive film has excellent nitrate detection performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene composite materials, and in particular to a preparation method of a graphene / nano copper composite conductive film and application thereof. Background Art

[0002] As a substance widely present in the natural environment, nitrate plays an important role in regulating soil fertility and maintaining crop growth. The content of nitrate in the soil is an important indicator, and the nitrate content plays an important role in indicating the quality of crop growth and the protection of the ecological environment. Too low nitrate content in the soil will lead to poor crop development, which will lead to low crop yields and affect agricultural income; too high nitrate content will cause crop seedlings to burn, which is also not conducive to crop growth. At the same time, excess nitrate will leave the soil and seep into groundwater, thereby polluting drinking water and aquatic systems, and bringing negative impacts to the ecological environment and human health. Therefore, taking effective measures to detect nitrate is crucial to improving crop growth, ensuring food production and protecting the ecological environment. The survey found that electrochemical sensors can effectively detect nitrates. However, traditional electrochemical sensors have limited the development of agriculture and the protection of the ecological environment to a certain extent due to their high cost and difficulty in manufacturing.

[0003] In view of this, it is necessary to design an improved preparation method of graphene / nano-copper composite conductive film and its application to solve the above problems. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a graphene / nano copper composite conductive film and application thereof.

[0005] To achieve the above-mentioned object of the invention, on the one hand, the present invention provides a method for preparing a graphene / nano copper composite conductive film, comprising the following steps:

[0006] S1, sequentially subjecting the graphene oxide film to carbonization treatment, annealing treatment and rolling compression to obtain a graphene film;

[0007] S2. Using the graphene film obtained in step S1 as a working electrode, a calomel electrode as a reference electrode, a platinum wire electrode as a counter electrode, and a copper salt solution as an electroplating solution, copper nanoparticles are deposited on the graphene film by electrochemical deposition to obtain a graphene / nano-copper composite conductive film.

[0008] Preferably, in step S1, the thickness of the graphene film is 400-500 μm.

[0009] Preferably, in step S1, the carbonization temperature is carried out at 1300-1400°C.

[0010] Preferably, in step S1, the annealing treatment is performed at 2000-2100°C.

[0011] Preferably, in step S1, the rolling compression is performed under the condition of 150-160 MPa.

[0012] Preferably, in step S1, the method for preparing the graphene oxide film is as follows: a graphene oxide suspension is stirred by mechanical stirring to form a graphene oxide gel, and then the graphene oxide gel is scraped to form a graphene oxide film; the graphene oxide suspension is prepared by dispersing graphene oxide in water, and its mass percentage is 4-5%.

[0013] Preferably, in step S2, the graphene film needs to be surface treated before electrodeposition, and the surface treatment is achieved by polishing the graphene film with sandpaper, and the sandpaper is fixed on a weight, the mass of the weight is 300g; the mesh size of the sandpaper is 100 mesh, 500 mesh or 1000 mesh.

[0014] Preferably, in step S2, the current density of the electrodeposition process is 2.5 mA / cm2, and the electrodeposition time is 1800 s.

[0015] In particular, the graphene / nano-copper composite conductive film prepared by the preparation method proposed in the present invention comprises a graphene film and copper nanoparticles deposited on the graphene film.

[0016] On the other hand, the graphene / nano copper composite conductive film prepared by the present invention can be applied to the field of electrochemical sensors, and is particularly suitable for further preparation into an electrochemical device for detecting nitrate.

[0017] The beneficial effects of the present invention are:

[0018] 1. The preparation method of the graphene / nano-copper composite conductive film provided by the present invention comprises the following steps: first preparing a graphene film, and then depositing copper nanoparticles on the graphene film by electrochemical deposition. This method can not only accurately control the deposition process of the copper nanoparticles, but also effectively increase the binding force between the copper nanoparticles and the graphene film, thereby ensuring that the copper nanoparticles are stably attached to the surface of the graphene film. The graphene / nano-copper composite conductive film prepared by the above method well maintains the softness and high conductivity of the graphene film itself.

[0019] 2. The preparation method of the graphene / nano-copper composite conductive film provided by the present invention is conducive to adjusting the surface structure of the graphene film by adopting a surface treatment method of sandpaper polishing, and forming a gully structure on the surface of the graphene film, which significantly increases the surface area of ​​the graphene film. The appearance of this structure increases the loading amount of copper nanoparticles, increases the active sites of electrochemical nitrate sensing, and enhances the detection performance of nitrate. The above process only requires simple mechanical polishing to achieve, has the advantages of simple, fast and efficient operation, and is conducive to large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a SEM image of the graphene film prepared in Example 1 of the present invention;

[0021] Figure 2 This is a SEM image of the surface-treated graphene film obtained in Example 4 of the present invention;

[0022] Figure 3 This is a SEM image of the graphene / nano-copper composite conductive film prepared in Example 4 of the present invention;

[0023] Figure 4 The cyclic voltammetry curves of the Cu / GF electrodes prepared in Examples 1 to 4 of the present invention at a concentration of 0.1 M sodium sulfate;

[0024] Figure 5 The current-time response curve of the Cu / GF electrode prepared in Example 4 of the present invention when potassium nitrate of different concentrations is continuously added at -1V;

[0025] Figure 6 This is a calibration curve of the current response and nitrate concentration of the Cu / GF electrode prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0027] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.

[0028] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0029] The method for preparing the graphene / nano copper composite conductive film provided by the present invention comprises the following steps:

[0030] S1, sequentially subjecting the graphene oxide film to carbonization treatment, annealing treatment and rolling compression to obtain a graphene film (GF);

[0031] S2. Using the graphene film obtained in step S1 as the working electrode, the calomel electrode as the reference electrode, the platinum wire electrode as the counter electrode, and the copper salt solution as the electroplating solution, copper nanoparticles are deposited on the graphene film by electrochemical deposition to obtain a graphene / nano-copper composite conductive film (Cu / GF).

[0032] As an embodiment of the present invention, in step S1, the preparation method of the graphene oxide film is as follows: a graphene oxide suspension is stirred by mechanical stirring to form a graphene oxide gel, and then the graphene oxide gel is scraped to form a graphene oxide film; wherein the graphene oxide suspension is prepared by dispersing graphene oxide in water, and its mass percentage is 4-5%.

[0033] As an embodiment of the present invention, in step S1, the carbonization treatment is carried out in a protective gas at 1300-1400° C. for 1-2 hours; the protective gas is argon or the like.

[0034] As an embodiment of the present invention, in step S1, the thickness of the graphene film is 400-500 μm.

[0035] As an embodiment of the present invention, in step S1, annealing treatment is performed at 2000-2100° C.; rolling compression is performed at 150-160 MPa.

[0036] As an embodiment of the present invention, in step S2, in order to facilitate the deposition of copper nanoparticles on the graphene film, the graphene film can be treated by surface treatment before electrodeposition. The surface treatment is completed by polishing the graphene film with sandpaper, and the sandpaper is fixed on a heavy object such as an iron block to speed up the work efficiency of the surface treatment. The mesh number of the sandpaper is 100 mesh, 500 mesh or 1000 mesh, preferably 100 mesh.

[0037] Through the above method, a groove structure can be formed on the surface of the graphene film, which is beneficial to increase the surface area of ​​the graphene film, increase the loading amount of copper nanoparticles, increase the sensing active sites in the subsequent electrochemical detection of nitrate, and enhance the detection performance of nitrate.

[0038] As an embodiment of the present invention, in step S2, the copper salt solution is a copper nitrate solution with a concentration of 10 mM.

[0039] As an embodiment of the present invention, in step S2, the current density of the electrodeposition process is 2.5 mA / cm 2 , the electrodeposition time is 1800s. In the above process, by adjusting the process parameters of the surface treatment, the amount of the loaded copper nanoparticles can be controlled to accurately adjust the performance of the graphene / nano-copper composite conductive film.

[0040] In particular, the graphene / nano copper composite conductive film prepared by the preparation method proposed in the present invention can be applied to electrochemical sensors, and is particularly suitable for further preparation into electrochemical devices for detecting nitrate, such as electrodes.

[0041] The preparation method and application of the graphene / nano copper composite conductive film provided by the present invention are further described below in conjunction with specific embodiments:

[0042] Example 1

[0043] This embodiment prepares a graphene / nano copper composite conductive film, and the specific preparation method includes the following steps:

[0044] S1. Graphene oxide is dispersed in deionized water to obtain a graphene oxide suspension with a mass percentage of 4%; the graphene oxide suspension is treated by ultrasound and stirring to obtain a graphene oxide gel, and the obtained product is scraped into a GO film of a certain thickness by scraping; then, the graphene oxide film is first slowly heated to 1300°C, kept warm for 1h in an argon atmosphere, and then the carbonized structure is annealed at 2000°C for 2h; finally, the sample is rolled and compressed at 150MPa to obtain GF; the SEM image of GF is shown in Figure 1 As shown, it can be seen from the figure that the surface of GF is relatively flat at the 300 μm scale;

[0045] S2. Cut the GF obtained in step S1 into a shape of 1 cm×2 cm and immerse it directly in an electroplating solution containing 10 mM copper nitrate solution (i.e., the GF is not surface treated). The area of ​​the graphene film immersed in the electroplating solution is 1 cm×1 cm. Then, place the electroplating solution on a magnetic stirrer, control the stirring speed to 100 rpm / min, use the GF without surface treatment as the working electrode, calomel as the auxiliary electrode, and platinum wire as the counter electrode, and use the three-electrode system of Chenhua 660E electrochemical workstation for electrochemical deposition. Use the chronoamperometry method and set the cathode current to 2.5 mA / cm 2 The cathode electrodeposition time was 1800s, and the anodic electrodeposition time was 0.005s, and Cu / GF which can be used as an electrode was obtained.

[0046] Cu / GF was subjected to cyclic voltammetry test to test the electrochemical activity of Cu / GF. During the test, Cu / GF electrode was used as the working electrode, platinum wire as the counter electrode, and calomel electrode as the reference electrode. The three-electrode system of Chenhua 660E electrochemical workstation was used for the test. The cyclic voltammetry scan range was -0.1V to -0.7V, and the scan rate was 50mV / S. During the test, 50mL of 0.1M sodium sulfate solution was set in the electrolytic cell to test the electrochemical activity of the electrode itself. The obtained cyclic voltammetry test graph is shown in the figure below. Figure 4 shown.

[0047] Example 2

[0048] This embodiment prepares a graphene / nano copper composite conductive film, and the specific preparation method includes the following steps:

[0049] S1. Graphene oxide is dispersed in deionized water to obtain a graphene oxide suspension with a mass percentage of 4%; the graphene oxide suspension is treated by ultrasound and stirring to obtain a graphene oxide gel, and the obtained product is scraped into a GO film of a certain thickness by scraping; then, the graphene oxide film is first slowly heated to 1300°C, kept warm for 1h in an argon atmosphere, and then the carbonized structure is annealed at 2000°C for 2h; finally, the sample is rolled and compressed at 150MPa to obtain GF; the SEM image of GF is shown in Figure 1 As shown, it can be seen from the figure that the surface of GF is relatively flat at the 300 μm scale;

[0050] S2, cutting the GF obtained in step S1 into a 1cm×2cm shape, immersing it in an electroplating solution containing 10mM copper nitrate solution after surface treatment, and the area of ​​the graphene film immersed in the electroplating solution is 1cm×1cm; then, placing the electroplating solution on a magnetic stirrer, controlling the stirring speed to 100rpm / min, using the surface-treated graphene film as the working electrode, calomel as the auxiliary electrode, and platinum wire as the counter electrode, using the three-electrode system of Chenhua 660E electrochemical workstation for electrochemical deposition, using the chronoamperometry, setting the cathode current to 2.5mA / cm 2 , the cathode electrodeposition time is 1800s, and the anode electrodeposition time is 0.005s, and Cu / GF that can be used as an electrode is obtained. Among them, the surface treatment is achieved by grinding the graphene film with 1000-mesh sandpaper, and the sandpaper is glued to the bottom of a 300g iron block. The grinding process is carried out as follows: the graphene film is laid flat on A4 paper, the sandpaper is placed flat on the graphene film, and the iron block is slowly pushed flat to make the sandpaper pass through the graphene film, and then the other side of the graphene film is laid flat on the A4 paper, and the flat pushing process is repeated to complete the surface treatment.

[0051] Cu / GF was subjected to cyclic voltammetry test to test the electrochemical activity of Cu / GF. During the test, Cu / GF electrode was used as the working electrode, platinum wire as the counter electrode, and calomel electrode as the reference electrode. The three-electrode system of Chenhua 660E electrochemical workstation was used for the test. The cyclic voltammetry scan range was -0.1V to -0.7V, and the scan rate was 50mV / S. During the test, 50mL of 0.1M sodium sulfate solution was set in the electrolytic cell to test the electrochemical activity of the electrode itself. The obtained cyclic voltammetry test graph is shown in the figure below. Figure 4 shown.

[0052] Example 3

[0053] This embodiment prepares a graphene / nano copper composite conductive film, and the specific preparation method includes the following steps:

[0054] S1. Graphene oxide is dispersed in deionized water to obtain a graphene oxide suspension with a mass percentage of 4%; the graphene oxide suspension is treated by ultrasound and stirring to obtain a graphene oxide gel, and the obtained product is scraped into a GO film of a certain thickness by scraping; then, the graphene oxide film is first slowly heated to 1300°C, kept warm for 1h in an argon atmosphere, and then the carbonized structure is annealed at 2000°C for 2h; finally, the sample is rolled and compressed at 150MPa to obtain GF; the SEM image of GF is shown in Figure 1 As shown, it can be seen from the figure that the surface of GF is relatively flat at the 300 μm scale;

[0055] S2, cutting the GF obtained in step S1 into a 1cm×2cm shape, immersing it in an electroplating solution containing 10mM copper nitrate solution after surface treatment, and the area of ​​the graphene film immersed in the electroplating solution is 1cm×1cm; then, placing the electroplating solution on a magnetic stirrer, controlling the stirring speed to 100rpm / min, using the surface-treated graphene film as the working electrode, calomel as the auxiliary electrode, and platinum wire as the counter electrode, using the three-electrode system of Chenhua 660E electrochemical workstation for electrochemical deposition, using the chronoamperometry, setting the cathode current to 2.5mA / cm 2 , the cathode electrodeposition time is 1800s, and the anode electrodeposition time is 0.005s, and Cu / GF that can be used as an electrode is obtained. Among them, the surface treatment is achieved by grinding the graphene film with 500-mesh sandpaper, and the sandpaper is glued to the bottom of a 300g iron block. The grinding process is carried out as follows: the graphene film is laid flat on A4 paper, the sandpaper is placed flat on the graphene film, and the iron block is slowly pushed flat to make the sandpaper pass through the graphene film, and then the other side of the graphene film is laid flat on the A4 paper, and the flat pushing process is repeated to complete the surface treatment.

[0056] Cu / GF was subjected to cyclic voltammetry test to test the electrochemical activity of Cu / GF. During the test, Cu / GF electrode was used as the working electrode, platinum wire as the counter electrode, and calomel electrode as the reference electrode. The three-electrode system of Chenhua 660E electrochemical workstation was used for the test. The cyclic voltammetry scan range was -0.1V to -0.7V, and the scan rate was 50mV / S. During the test, 50mL of 0.1M sodium sulfate solution was set in the electrolytic cell to test the electrochemical activity of the electrode itself. The obtained cyclic voltammetry test graph is shown in the figure below. Figure 4 shown.

[0057] Example 4

[0058] This embodiment prepares a graphene / nano copper composite conductive film, and the specific preparation method includes the following steps:

[0059] S1. Graphene oxide is dispersed in deionized water to obtain a graphene oxide suspension with a mass percentage of 4%; the graphene oxide suspension is treated by ultrasound and stirring to obtain a graphene oxide gel, and the obtained product is scraped into a GO film of a certain thickness by scraping; then, the graphene oxide film is first slowly heated to 1300°C, kept warm for 1h in an argon atmosphere, and then the carbonized structure is annealed at 2000°C for 2h; finally, the sample is rolled and compressed at 150MPa to obtain GF; the SEM image of GF is shown in Figure 1 As shown, it can be seen from the figure that the surface of GF is relatively flat at the 300 μm scale;

[0060] S2, cutting the GF obtained in step S1 into a 1cm×2cm shape, immersing it in an electroplating solution containing 10mM copper nitrate solution after surface treatment, and the area of ​​the graphene film immersed in the electroplating solution is 1cm×1cm; then, placing the electroplating solution on a magnetic stirrer, controlling the stirring speed to 100rpm / min, using the surface-treated graphene film as the working electrode, calomel as the auxiliary electrode, and platinum wire as the counter electrode, using the three-electrode system of Chenhua 660E electrochemical workstation for electrochemical deposition, using the chronoamperometry, setting the cathode current to 2.5mA / cm 2 , the cathode electrodeposition time is 1800s, and the anode electrodeposition time is 0.005s, and Cu / GF that can be used as an electrode is obtained. Among them, the surface treatment is achieved by grinding the graphene film with 100-mesh sandpaper, and the sandpaper is glued to the bottom of a 300g iron block. The grinding process is carried out as follows: the graphene film is laid flat on A4 paper, the sandpaper is placed flat on the graphene film, and the iron block is slowly pushed flat to make the sandpaper pass through the graphene film, and then the other side of the graphene film is laid flat on the A4 paper, and the flat pushing process is repeated to complete the surface treatment. The SEM image of the GF after surface treatment is shown in Figure 2As shown in the figure, it can be clearly seen that there are obvious grooves on the surface of the treated film; the SEM image of Cu / GF is shown in Figure 3 As shown, it can be seen that except for a small number of copper nanoparticles that have aggregated, the copper nanoparticles are deposited relatively evenly on the surface of the graphene film, and the particle size of the copper nanoparticles is 500nm-800nm.

[0061] Cu / GF was subjected to cyclic voltammetry test to test the electrochemical activity of Cu / GF. During the test, Cu / GF electrode was used as the working electrode, platinum wire as the counter electrode, and calomel electrode as the reference electrode. The three-electrode system of Chenhua 660E electrochemical workstation was used for the test. The cyclic voltammetry scan range was -0.1V to -0.7V, and the scan rate was 50mV / S. During the test, 50mL of 0.1M sodium sulfate solution was set in the electrolytic cell to test the electrochemical activity of the electrode itself. The cyclic voltammetry curve of Cu / GF at 0.1M sodium sulfate concentration is shown in the figure below. Figure 4 As shown, the results show that surface treatment can improve the electrochemical properties of the composite film, among which the performance is best after surface treatment with 100-mesh sandpaper. The principle is that the graphene film surface treated with 100-mesh sandpaper has a larger surface area than the 500-mesh, 1000-mesh and untreated graphene film surfaces. Therefore, more copper nanoparticles are electrochemically deposited on the surface, and its electrochemical activity is stronger.

[0062] The current-time curve test was used to test the effect of adding different concentrations of potassium nitrate on the current. During the Cu / GF test, 50mL of 0.1M sodium sulfate was set as the supporting electrolyte in the electrolytic cell, and different concentrations of potassium nitrate were added to the electrolytic cell. During the test, the electrolytic cell was placed on a magnetic stirring table for stirring, and the working voltage was set to -1V to explore the relationship between the test current and the nitrate concentration. The detection process is implemented according to the following mechanism: NO3 - +10H + 8e - →NH4 + +3H2O.

[0063] The amperometric response curve of Cu / GF at -1V when adding different concentrations of potassium nitrate continuously is shown in the figure. Figure 5 As shown in Figure 2, it can be seen that under the catalytic action of Cu / GF, the current increases with the addition of nitrate, and the detectable concentration range of nitrate is 0-299.1 μM; the calibration curve of the current response of Cu / GF and the nitrate concentration is shown in Figure 2 Figure 6 As shown in the figure, it can be seen that there is an obvious linear relationship between the two. The relevant linear equation obtained by calculation is: y = 0.64C NO3 -+1080.88, where the linear correlation coefficient R 2The value of Cu / GF electrode was 0.989, and the sensitivity of Cu / GF electrode in detecting glucose was calculated to be 0.64μA / μM. The detection limit was calculated to be 7.5μM by the standard deviation and slope (S / N=3) of the calibration curve with a confidence factor of 3. The results show that the Cu / GF prepared by the preparation method proposed by the present invention has excellent nitrate detection performance. The calculation formula of the detection limit is LOD=3δ / S, where δ represents the standard deviation of the calibration curve and S represents the slope of the calibration curve.

[0064] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a graphene / nano copper composite conductive film, characterized in that: The steps include: S1, sequentially subjecting the graphene oxide film to carbonization treatment, annealing treatment and rolling compression to obtain a graphene film; S2. Using the graphene film obtained in step S1 as a working electrode, a calomel electrode as a reference electrode, a platinum wire electrode as a counter electrode, and a copper salt solution as an electroplating solution, copper nanoparticles are deposited on the graphene film by electrochemical deposition to obtain a graphene / nano-copper composite conductive film.

2. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S1, the thickness of the graphene film is 400-500 μm.

3. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S1, the annealing treatment is performed at 2000-2100°C.

4. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S1, the rolling compression is performed under the condition of 150-160 MPa.

5. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S1, the preparation method of the graphene oxide film is as follows: a graphene oxide suspension is stirred by mechanical stirring to form a graphene oxide gel, and then the graphene oxide gel is scraped to form a graphene oxide film; the graphene oxide suspension is prepared by dispersing graphene oxide in water, and its mass percentage is 4-5%.

6. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S2, the graphene film needs to be surface treated before electrodeposition, and the surface treatment is achieved by polishing the graphene film with sandpaper, and the sandpaper is fixed on a weight, the mass of the weight is 300g; the mesh size of the sandpaper is 100 mesh, 500 mesh or 1000 mesh.

7. The method for preparing the graphene / nano copper composite conductive film according to claim 1, characterized in that: In step S2, the current density of the electrodeposition process is 2.5 mA / cm 2 , the electrodeposition time is 1800s.

8. A graphene / nano copper composite conductive film prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The invention comprises a graphene film and copper nanoparticles deposited on the graphene film.

9. Application of a graphene / nano-copper composite conductive film in an electrochemical sensor.

10. An electrochemical device for detecting nitrate, characterized in that: The electrochemical device comprises a graphene / nano copper composite conductive film.