Roadbed filling method for modifying poor clay through industrial waste residues
By using specific proportions of phosphogypsum, admixtures and slaked lime in highway subgrade filling, improved soil is formed, which solves the problem of subgrade stability caused by poor clay and achieves high-strength, low-cost and environmentally friendly filling effects.
Patent Information
- Application Number
- CN202411009970.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-10-08
AI Technical Summary
In highway subgrade filling, undesirable clay such as expansive soil and red clay leads to shrinkage and cracking of the subgrade, and the direct use of cement and lime doped methods is costly and difficult to achieve ideal results in terms of strength and economic benefits.
The ratio of phosphogypsum, admixture and slaked lime is 1:0.1:0.02~0.025. Stir evenly through the mixing station and then add water to form a phosphogypsum composite. Spread it on the clay surface and mix it. Let it stand, level it and vibrate it. Pressure, control the optimal moisture content to improve the strength and stability of the improved soil.
It significantly improves the bearing ratio and water stability of the improved soil, meets the highway fill performance requirements, reduces costs and environmental pollution, and achieves the dual advantages of economic and environmental benefits.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road construction, in particular to a roadbed filling method for transforming poor clay with industrial waste residue. Background Art
[0002] During the construction of highway subgrade, you may encounter undesirable clay, such as expansive soil and red clay. Expansive soil has the characteristics of swelling when absorbing water and shrinking when losing water, which can easily cause shrinkage and cracking of the subgrade, destroying the strength and stability of the subgrade. High liquid limit red clay has low compressibility and high shear strength in its natural state, but after being soaked in water, it has high water content and low strength. It has the characteristics of being hard on the top and soft on the bottom, strong water sensitivity, shrinking when losing water, developing cracks, and being easy to deform and become unstable.
[0003] For poor clay roadbed filling materials such as expansive soil and red clay, the soil properties can usually be improved by adding crushed stone, cement, lime, fly ash, etc., and the adverse effects can be eliminated by reasonably controlling its rolling moisture content and dry density. However, directly using cement and lime and other materials mixed with poor clay for roadbed filling will increase costs because the amount of cement and lime and other materials used is relatively large.
[0004] Therefore, how to provide a roadbed filling method for transforming poor clay with industrial waste residue, and how to use industrial waste residue to transform poor clay for roadbed filling to achieve high economic and environmental benefits under the premise of high strength and stable volume, is a technical problem that technical personnel in this field urgently need to solve. Summary of the invention
[0005] In view of the problems existing in the prior art, the technical problem to be solved by the present invention is to provide a roadbed filling method for transforming poor clay with industrial waste residues. Using industrial waste residues to transform poor clay for roadbed filling can achieve high economic and environmental benefits under the premise of high strength and stable volume.
[0006] To achieve the above-mentioned purpose, the present invention provides a roadbed filling method for transforming poor clay with industrial waste residues, and the roadbed filling method for transforming poor clay with industrial waste residues comprises: S1, using a mixing station to evenly mix phosphogypsum, admixtures, and slaked lime to obtain a mixture, and then adding water to the mixture while mixing it with a mixing station until the mixture is loose and moist, to obtain a phosphogypsum composite; S2, spreading clay on the filling site, and then spreading the phosphogypsum composite on the surface of the clay, mixing the spread clay and the spread phosphogypsum composite 3 to 4 times by a road mixer to obtain improved soil, and then covering the improved soil with a film and letting it stand for 24 hours; S3, leveling the improved soil after standing at the filling site, and then rolling it with a vibrating roller until the compaction requirement is met, and the filling is completed.
[0007] In the first aspect: the mass ratio of phosphogypsum, admixture and slaked lime in S1 is 1:0.1:0.02-0.025.
[0008] In the first aspect, the mass ratio of the clay in S2 to the phosphogypsum in S1 is 1:0.42-0.48.
[0009] In the first aspect, the moisture content of the improved soil obtained in S2 is controlled to be 1% to 2% above the optimum moisture content; the moisture content of the improved soil in S3 is controlled to be 1% to 2% above the optimum moisture content during rolling.
[0010] In the first aspect, the test method for the optimal moisture content specifically includes: mixing clay, phosphogypsum, admixture and slaked lime in proportion to obtain improved soil, dividing the improved soil into no less than 5 groups by mass, adding different masses of water to each group of the improved soil, and obtaining no less than 5 groups of improved soil with a moisture content of 18% as a base point and an interval of 2%, performing compaction tests on the improved soils to obtain the dry density corresponding to each group of the improved soils, and drawing a curve chart of the relationship between moisture content and dry density. The moisture content at the peak point of the curve of the relationship between moisture content and dry density is the optimal moisture content of the improved soil; the mass ratio of the phosphogypsum, admixture and slaked lime is the same as the mass ratio of the phosphogypsum, admixture and slaked lime in S1, and the mass ratio of the clay and phosphogypsum is the same as the mass ratio of the clay in S2 and the phosphogypsum in S1.
[0011] In the first aspect, after the S3 is filled, watering and curing is continued for 7 days on the surface of the compacted layer of the improved soil.
[0012] In the first aspect, the calcium sulfate content in the phosphogypsum is not less than 75%; and the pH of the phosphogypsum is 7-9.
[0013] In the first aspect, the admixture comprises one or more of granulated blast furnace slag powder, fly ash and pozzolan, and the pozzolan activity index of the admixture at 28 days is not less than 75%.
[0014] In the first aspect, the slaked lime is calcareous slaked lime, and the grade of the slaked lime is HCL75 and above.
[0015] In the first aspect, the clay includes one or more of swelling clay, high liquid limit clay and red clay.
[0016] Beneficial effects:
[0017] The improved soil is obtained by mixing clay, phosphogypsum, admixture and slaked lime according to a mass ratio of phosphogypsum, admixture and slaked lime of 1:0.1:0.02-0.025 and a mass ratio of clay to phosphogypsum of 1:0.42-0.48. This ratio can effectively stimulate the activity of the admixture, phosphogypsum, slaked lime and clay, so that the strength index bearing ratio (CBR) of the improved soil is increased to more than 10 times that of clay, so that the load expansion rate meets the requirements of non-expansive soil, and can meet the performance requirements of highway roadbed filling.
[0018] Using a mixing station to mix the phosphogypsum composite separately in advance is beneficial to the precise control of the amount of each component in the phosphogypsum composite; making the phosphogypsum composite loose and non-clumping can ensure smooth feeding during the subsequent paving process and easy dispersion during mixing, which is beneficial to shortening the construction time and increasing mixing uniformity; covering the improved soil with a film and letting it stand for 24 hours can prevent the moisture in the improved soil from evaporating outwards, allowing the water molecules to fully diffuse in the improved soil, increasing the uniformity of water distribution in the improved soil, and helping to improve the compaction density. The spread clay and phosphogypsum composite material is mixed 3 to 4 times with a lime soil road mixer to break up the large lumps in the clay and phosphogypsum composite material into small particles, making the clay and phosphogypsum composite material mixed more evenly, and then compacted with a vibrating roller according to the predetermined process parameters and the compaction degree meets the requirements, which can ensure that the clay and phosphogypsum composite material is mixed evenly, make the various components in the improved soil evenly distributed and in close contact, promote the occurrence of related physical and chemical reactions, and be beneficial to the compaction of the improved soil roadbed, prevent moisture intrusion, and improve the bearing ratio, water stability and volume stability of the roadbed.
[0019] Phosphogypsum is a solid waste discharged by phosphate mining enterprises, and its stockpile is large. The present invention uses phosphogypsum to transform poor clay to obtain improved soil. The mass ratio of clay to phosphogypsum in the improved soil is 1:0.42-0.48, so that the amount of phosphogypsum in each cubic meter of improved soil is as high as 500kg. It is widely used in highway roadbeds, can have a large absorption capacity for phosphogypsum, reduce the land occupation and environmental pollution caused by the accumulation of phosphogypsum, and the large-scale use of phosphogypsum also reduces the consumption of clay and saves land resources. The used phosphogypsum is washed with water and pre-treated with alkali, and the concentration of harmful components in the leachate does not exceed the limit value specified in relevant specifications, so it is environmentally friendly. First, a mixing station is used to evenly stir the phosphogypsum, admixtures, slaked lime and an appropriate amount of water, so that the mixture is loose and moist, and a phosphogypsum composite is obtained. The loose and moist state can effectively reduce the pollution of the environment caused by dust stirred up during the mixing, transportation and paving of the phosphogypsum composite.
[0020] As a solid waste, phosphogypsum has a material cost close to zero, and the government has corresponding subsidies for its disposal. Although the admixtures and slaked lime in the improved soil have material costs, the amount used is very small. Compared with traditional soil improvement methods, the overall cost is low and the economic benefits are significant. The amount of phosphogypsum composite is small, and the amount of clay is large. The phosphogypsum composite is mixed separately using a mixing station, and the clay and phosphogypsum composite is mixed on the roadbed using a road mixer. Compared with the practice of mixing all the components of the improved soil using a mixing station, it can save the transportation and mixing costs of clay between the mixing station and the roadbed, and shorten the working hours.
[0021] In summary, the roadbed filling method of transforming poor clay with industrial waste residue of the present invention can improve the bearing ratio, water stability and volume stability of the roadbed, while reducing costs and absorbing solid waste, which has significant environmental and economic benefits. DETAILED DESCRIPTION
[0022] The technical solutions in the embodiments of this specification are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of this specification, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the embodiments in this specification belong to the scope of protection of the present invention.
[0023] Embodiment 1
[0024] The first embodiment provides a method for roadbed filling of poor clay transformed by industrial waste residues, and the method comprises: S1, using a mixing station to evenly mix phosphogypsum, admixtures, and slaked lime to obtain a mixture, and then adding water to the mixture while mixing it with a mixing station until the mixture is loose and moist, to obtain a phosphogypsum composite; S2, spreading clay on the filling site, and then spreading the phosphogypsum composite on the surface of the clay, and using a road mixer to spread the phosphogypsum composite on the clay surface. The good clay and the spread phosphogypsum composite material are mixed 3 to 4 times to obtain improved soil, and then a film is covered on the improved soil and allowed to stand for 24 hours; S3, the improved soil after standing is leveled at the filling site, and then rolled with a vibrating roller until the compaction requirements are met, and the filling is completed; the mass ratio of the phosphogypsum, admixture and slaked lime in S1 is 1:0.1:0.02-0.025; the mass ratio of the clay in S2 to the phosphogypsum in S1 is 1:0.42-0.48.
[0025] The improved soil is obtained by mixing clay, phosphogypsum, admixture and slaked lime according to a mass ratio of phosphogypsum, admixture and slaked lime of 1:0.1:0.02-0.025 and a mass ratio of clay to phosphogypsum of 1:0.42-0.48. This ratio can effectively stimulate the activity of the admixture, phosphogypsum, slaked lime and clay, so that the strength index bearing ratio (CBR) of the improved soil is increased to more than 10 times that of clay, so that the load expansion rate meets the requirements of non-expansive soil, and can meet the performance requirements of highway roadbed filling.
[0026] Using a mixing station to mix and combine the phosphogypsum composite separately is beneficial to the precise control of the amount of each component in the phosphogypsum composite; making the phosphogypsum composite loose and non-clumping can ensure smooth feeding during the subsequent paving process and easy dispersion during mixing, which is beneficial to shortening the construction time and increasing mixing uniformity; covering the improved soil with a film and letting it stand for 24 hours to seal the material can prevent the moisture in the improved soil from evaporating outwards, allowing the water molecules to fully diffuse in the improved soil, increasing the uniformity of water distribution in the improved soil, and helping to improve the compaction density. The spread clay and phosphogypsum composite material is mixed 3 to 4 times with a lime soil road mixer to break up the large lumps in the clay and phosphogypsum composite material into small particles, making the clay and phosphogypsum composite material mixed more evenly, and then compacted with a vibrating roller according to the predetermined process parameters and the compaction degree meets the requirements, which can ensure that the clay and phosphogypsum composite material is mixed evenly, make the various components in the improved soil evenly distributed and in close contact, promote the occurrence of related physical and chemical reactions, and be beneficial to the compaction of the improved soil roadbed, prevent moisture intrusion, and improve the bearing ratio, water stability and volume stability of the roadbed.
[0027] Phosphogypsum is a solid waste discharged by phosphate mining enterprises, and its stockpile is large. The present invention uses phosphogypsum to transform poor clay, and the mass ratio of clay to phosphogypsum in the improved soil is 1:0.42-0.48, so that the amount of phosphogypsum in each cubic meter of improved soil is as high as 500kg. It is widely used in highway roadbeds, and can have a large absorption capacity for phosphogypsum, reduce the land occupation and environmental pollution caused by the accumulation of phosphogypsum, and the large-scale use of phosphogypsum also reduces the consumption of clay and saves land resources. The used phosphogypsum is pre-treated by water washing and alkali addition, and the concentration of harmful components in the leachate does not exceed the limit value specified in relevant specifications, and it is environmentally friendly. First, a mixing station is used to evenly stir the phosphogypsum, admixtures, slaked lime and an appropriate amount of water, so that the mixture is loose and moist, and a phosphogypsum composite is obtained. The loose and moist state can effectively reduce the pollution of the environment caused by dust stirred up during the mixing, transportation and paving of the phosphogypsum composite.
[0028] As a solid waste, phosphogypsum has a material cost close to zero, and the government has corresponding subsidies for its disposal. Although the admixtures and slaked lime in the improved soil have material costs, the amount used is very small. Compared with traditional soil improvement methods, the overall cost is low and the economic benefits are significant. The amount of phosphogypsum composite is small, and the amount of clay is large. The phosphogypsum composite is mixed separately using a mixing station, and the clay and phosphogypsum composite is mixed on the roadbed using a road mixer. Compared with the practice of mixing all the components of the improved soil using a mixing station, it can save the transportation and mixing costs of clay between the mixing station and the roadbed, and shorten the working hours.
[0029] In summary, the roadbed filling method of transforming poor clay with industrial waste residue of the present invention can improve the bearing ratio, water stability and volume stability of the roadbed, while reducing costs and absorbing solid waste, which has significant environmental and economic benefits.
[0030] In some possible implementations, the moisture content of the improved soil obtained in S2 is controlled to be 1% to 2% above the optimal moisture content; and the moisture content of the improved soil in S3 is controlled to be 1% to 2% above the optimal moisture content during rolling.
[0031] Specifically, water will be lost during the spreading of clay and phosphogypsum composite materials. To compensate for the lost water, the water content is increased based on the optimum water content. Therefore, the water content of the improved soil obtained in S2 is required to be 1% to 2% above the optimum water content. In addition, water will be lost during the rolling of the improved soil. To compensate for the lost water, the water content is increased based on the optimum water content. Therefore, the water content of the improved soil in S3 is required to be controlled at 1% to 2% above the optimum water content during rolling.
[0032] In some possible implementations, the test method for the optimal moisture content specifically includes: the test method for the optimal moisture content specifically includes: mixing clay, phosphogypsum, admixture and slaked lime in proportion to obtain improved soil, dividing the improved soil into no less than 5 groups according to mass, adding different masses of water to each group of the improved soil, to obtain no less than 5 groups of improved soil with a moisture content of 18% as a base point and an interval of 2%, subjecting the improved soils to compaction tests to obtain the dry density corresponding to each group of the improved soil, and drawing a curve chart of the relationship between moisture content and dry density, the moisture content at the peak point of the curve of the relationship between moisture content and dry density is the optimal moisture content of the improved soil; the mass ratio of the phosphogypsum, admixture and slaked lime is the same as the mass ratio of the phosphogypsum, admixture and slaked lime in S1, and the mass ratio of the clay and phosphogypsum is the same as the mass ratio of the clay in S2 and the phosphogypsum in S1.
[0033] Specifically, the improved soil is prepared according to the requirements of clay, phosphogypsum, admixtures, slaked lime and water in the roadbed filling method of transforming poor clay from industrial waste, and the optimal moisture content of the improved soil will be around 18%. Therefore, taking 18% as the base point and setting no less than 5 moisture contents at intervals of 2% for compaction tests can more easily cover the optimal moisture content within the set moisture content range, thereby shortening the time of the test work and saving costs.
[0034] In some possible implementations, after the S3 is filled, water is sprinkled on the surface of the compacted layer of the improved soil for 7 days for maintenance.
[0035] Specifically, proper watering and maintenance after filling can not only keep the compacted improved soil moist to a certain degree and allow the active reaction in the improved soil to continue; it can also prevent the surface of the improved soil roadbed from shrinking and cracking after water loss.
[0036] In some possible implementations, the calcium sulfate content in the phosphogypsum is not less than 75%; and the pH of the phosphogypsum is 7-9.
[0037] Specifically, the calcium sulfate content in phosphogypsum is not less than 75%, which can ensure that phosphogypsum can provide enough sulfate ions and calcium ions, thereby improving the strength of the roadbed filled with improved soil; phosphogypsum needs to be pre-treated with water washing and alkali doping. After water washing and alkali doping, the phosphogypsum is weakly alkaline, which promotes the stimulation of material activity in the improved soil and can improve the strength of the roadbed filled with improved soil; in addition, after the phosphogypsum is pre-treated with water washing and alkali doping, the concentration of harmful components in the leachate of the phosphogypsum does not exceed the limit value specified in the relevant specifications, so that the phosphogypsum will not be damaged due to excessive harmful components after being used for the roadbed. Pollution to the environment; furthermore, in the process of mixing the phosphogypsum composite material at the mixing station, the phosphogypsum lumps with a particle size greater than 15 mm in the phosphogypsum composite material are broken up into phosphogypsum lumps with a particle size not greater than 15 mm, so that the phosphogypsum is in full contact with other materials of the improved clay and with the clay, promoting the occurrence of physical and chemical effects of the phosphogypsum, thereby improving the strength of the roadbed filled with improved soil, and at the same time, avoiding the problem of requiring the lumps to have a particle size that is too small and thus increasing the crushing cost too much, and avoiding the problem of increasing the crushing cost by crushing the lumps larger than 15 mm in advance because the lumps to be added have a particle size of no more than 15 mm.
[0038] In some possible implementations, the admixture includes one or more of granulated blast furnace slag powder, fly ash and pozzolan, and the pozzolan activity index of the admixture at 28 days is not less than 75%.
[0039] Specifically, the volcanic ash activity index of the admixture at 28 days is not less than 75%, so that there are enough active substances in the improved soil, thereby improving the strength, water stability and volume stability of the roadbed filled with improved soil.
[0040] In some possible implementations, the slaked lime is calcareous slaked lime, and the grade of the slaked lime is HCL75 and above.
[0041] Specifically, the slaked lime is calcium slaked lime of HCL75 or above, so that there are enough active substances in the improved soil, which improves the strength, water stability and volume stability of the roadbed filled with improved soil.
[0042] In some possible implementations, the clay includes one or more of swelling clay, high liquid limit clay and red clay.
[0043] Specifically, in the process of mixing clay and phosphogypsum composite materials by using a road mixer, the road mixer will break up clay lumps with a particle size greater than 15 mm into clay lumps with a particle size no greater than 15 mm, so that the clay is in full contact with the phosphogypsum, admixtures and slaked lime, and the physical and chemical reactions between the clay and the phosphogypsum, admixtures and slaked lime are promoted, thereby improving the strength of the roadbed filled with improved soil. At the same time, it avoids the problem of requiring the particle size of the lumps to be too small and thus increasing the crushing cost too much, and avoids the problem of increasing the crushing cost by crushing lumps larger than 15 mm in advance because the particle size of the lumps to be added is no greater than 15 mm.
[0044] In order to further illustrate the technical solution of the present application in detail to support the technical problem to be solved by the present application, the implementation method is described below with specific examples, such as Example 1.
[0045] Example 1
[0046] Background: There is expansive soil in the route area of a highway construction project, which needs to be improved for roadbed filling, and the required processing volume is 10 million cubic meters; there are many phosphorus chemical companies near the project, and the total stockpile of phosphogypsum discharged by them exceeds 30 million tons. The test result of calcium sulfate content in phosphogypsum is 90.1%. It was washed and doped with alkali before storage, and the pH value is 8.0. The concentration of harmful components in the leachate does not exceed the limit specified in the relevant specifications, and there is no environmental pollution risk. In addition, due to long-term accumulation, there are consolidated lumps in the phosphogypsum pile, and the particle size is far more than 15mm. In addition, in order to protect the environment, the local government has introduced a policy to encourage the consumption of phosphogypsum, with a subsidy of 20 yuan for every ton of phosphogypsum consumed, and the total subsidy amount for a single project does not exceed 5 million yuan. The phosphorus chemical company promised that if phosphogypsum is used for roadbed filling, it will be delivered to the construction site free of charge.
[0047] raw material:
[0048] Expansive soil: The expansive soil in the background of Example 1 is transferred from the roadbed excavation section to the filling section. There are clumps with a particle size greater than 15 mm, which will be broken up during mixing in the road mixer.
[0049] Phosphogypsum: At the storage point of phosphogypsum in the context of Example 1, there are lumps with a particle size greater than 15 mm, which need to be broken up during mixing at the mixing station.
[0050] Granulated blast furnace slag powder: The pozzolanic activity index at 28d age is 82%.
[0051] HCL75 Calcium slaked lime: Calcium oxide plus magnesium oxide content is 80%
[0052] A roadbed filling method for transforming poor clay with industrial waste residue specifically comprises:
[0053] Expansive soil, phosphogypsum, granulated blast furnace slag powder and HCL75 calcium slaked lime were mixed in a mass ratio of 10:4.5:0.45:0.1 to obtain improved soil, and the improved soil was divided into five groups according to mass. Different masses of water were added to the five groups of improved soil to obtain five groups of improved soil with water contents of 14%, 16%, 18%, 20% and 22%, respectively. After the five groups of improved soil were covered with plastic film and left to stand for 24 hours, compaction tests were performed on the five groups of improved soil to obtain the corresponding dry densities of the five groups of improved soil, and a relationship curve between moisture content and dry density was drawn. The optimal moisture content of the improved soil was 18.6%, and the maximum dry density was 1730kg / m 3 .
[0054] Using a mixing station, phosphogypsum, granulated blast furnace slag powder and HCL75 calcium slaked lime are uniformly mixed in a mass ratio of 4.5:0.45:0.1 to obtain a mixture, and then water is added to the mixture while mixing it with the mixing station until the mixture is loose and moist to obtain a phosphogypsum composite material;
[0055] Testing the moisture content of the expansive soil and phosphogypsum composite, calculating the moisture content of the expansive soil and phosphogypsum composite after mixing according to the moisture content of the expansive soil and phosphogypsum composite, if the calculated moisture content of the expansive soil and phosphogypsum composite after mixing is higher than 20.6%, turning and drying the expansive soil until the moisture content of the expansive soil and phosphogypsum composite after turning and drying is lower than 20.6%;
[0056] Determine the loose paving thickness to be 30 mm, the mass ratio of expansive soil to phosphogypsum to be 10:4.5, calculate the amount of expansive soil and phosphogypsum composite material in the current filling layer based on the filling area and loose paving thickness, then spread the expansive soil on the filling site, then spread the phosphogypsum composite material on the surface of the expansive soil, mix the spread expansive soil and the spread phosphogypsum composite material 4 times with a road mixer to obtain improved soil, and then cover the improved soil with plastic film and let it stand for 24 hours;
[0057] The improved soil after being left to stand is leveled at the filling position, and the moisture content of the improved soil is tested. If the moisture content is less than 19.6%, water is sprinkled on the improved soil until the moisture content of the improved soil is between 19.6% and 20.6%. Then, a 16-ton vibrating roller is used to firstly perform static rolling for 2 times, then perform vibration rolling for 4 times, and then perform static rolling for 2 times, so that the compaction degree is not less than 96%, and the filling is completed;
[0058] After filling, the surface of the compacted layer of improved soil was watered for 7 days for maintenance, thus obtaining the transformation of poor clay roadbed with industrial waste residue.
[0059] The roadbed performance of the poor clay transformed from industrial waste prepared in Example 1 is as follows:
[0060] CBR and load expansion rate test:
[0061] Referring to the T0134-2019 bearing ratio (CBR) test and T0126-1993 load expansion rate test in the "Highway Geotechnical Test Code" JTG 3430-2020, the CBR and load expansion rate of the poor clay roadbed transformed by industrial waste residue in Example 1 were tested respectively, and the test data are shown in Table 1.
[0062] Table 1 CBR and load expansion rate test data
[0063] Example CBR Expansion rate under load Example 1 60% 0.5%
[0064] As shown in Table 1, the CBR of the poor clay roadbed transformed by industrial waste slag in Example 1 is 60.4%, the load expansion rate is 0.5%, the strength is high, the volume is stable, and the engineering quality requirements are met. At the same time, the CBR of the poor clay roadbed transformed by industrial waste slag in Example 1 is increased by 10 times compared with the CBR of the roadbed directly filled with expansive soil, the volume is stable, and the engineering quality requirements are met.
[0065] Economic benefits:
[0066] According to Example 1, the improved soil is obtained by mixing expansive soil, phosphogypsum, granulated blast furnace slag powder and HCL75 calcium slaked lime in a mass ratio of 10:4.5:0.45:0.1. The phosphogypsum discharged and stockpiled by phosphorus chemical enterprises is used to mix the expansive soil, which saves the cost of purchasing phosphogypsum. At the same time, the government also subsidizes the project of disposing of phosphogypsum, which reduces part of the cost while saving the cost of purchasing phosphogypsum. Compared with the cost of improved soil obtained by traditional method of adding 80kg of HCL75 calcium slaked lime into each cubic meter of expansive soil, the cost of each cubic meter of improved soil of the present invention saves about 15 yuan, and the economic benefit is significant.
[0067] Environmental benefits:
[0068] According to Example 1, the improved soil is obtained by mixing expansive soil, phosphogypsum, granulated blast furnace slag powder and HCL75 calcium slaked lime in a mass ratio of 10:4.5:0.45:0.1. It can be seen that each cubic meter of improved soil absorbs 508 kg of phosphogypsum, and the amount of phosphogypsum solid waste absorbed is large, which reduces solid waste accumulation and environmental pollution. In addition, the content of hazardous components in the phosphogypsum used is far lower than the relevant requirements, and the environmental benefits are significant.
[0069] In summary, the phosphogypsum composite material is obtained by mixing phosphogypsum, granulated blast furnace slag powder and HCL75 calcium slaked lime at a mass ratio of 4.5:0.45:0.1 using a mixing station and then adding appropriate amount of water to mix. During the mixing process, large-size agglomerates are broken into small agglomerates with a particle size of less than 15 mm, which saves costs, promotes the physical and chemical effects of phosphogypsum in the subsequent rolling process, and improves the strength, water stability and volume stability of the improved soil fill roadbed. The phosphogypsum composite material is mixed with water to reduce dust pollution during transportation and subsequent paving of the phosphogypsum composite material; after paving the expansive soil, the phosphogypsum composite material is spread on the expansive soil, the mass ratio of the expansive soil to the phosphogypsum in the phosphogypsum composite material is 10:4.5, and then the road mixer is used to mix directly to ensure that the moisture content of the improved soil after mixing is 1% to 2% higher than the optimal moisture content obtained by the test, while avoiding dust pollution in the subsequent construction process and avoiding the mixing of the expansive soil and the phosphogypsum composite material. The increase in the transportation cost of expansive soil caused by mixing at the mixing station saves costs; phosphogypsum is a solid waste, which reduces the cost of raw materials; phosphogypsum accounts for a large proportion in the improved soil, which increases the consumption of phosphogypsum solid waste and reduces the accumulation of solid waste; at the same time, in the process of rolling the improved soil to form a roadbed, phosphogypsum, expansive soil, granulated blast furnace slag powder and HCL75 calcium slaked lime are fully in contact, and the granulated blast furnace slag powder shows good activity under the stimulation of HCL75 calcium slaked lime, and has complex physical and chemical reactions with calcium ions, sulfate ions in phosphogypsum and silicon dioxide in expansive soil, thereby showing the improvement of the strength, water stability and volume stability of the roadbed filled with improved soil. Compared with the roadbed directly filled with expansive soil, its CBR value is increased by about 10 times; the improved soil filling roadbed of the present invention not only has good economic benefits but also good environmental benefits. At the same time, the roadbed obtained by the improved soil filling of the present invention is not only high in strength, but also has good water stability and volume stability. The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A roadbed filling method for transforming poor clay with industrial waste residue, characterized in that: The roadbed filling method for transforming poor clay with industrial waste residues comprises: S1. Using a mixing station, the phosphogypsum, admixture, and slaked lime are uniformly stirred to obtain a mixture, and then water is added to the mixture while stirring with the mixing station until the mixture is loose and moist, to obtain a phosphogypsum composite; S2, spreading clay on the filling site, and then spreading the phosphogypsum composite material on the surface of the clay, mixing the spread clay and the spread phosphogypsum composite material 3 to 4 times by a road mixer to obtain improved soil, and then covering the improved soil with a film and leaving it to stand for 24 hours; S3, leveling the improved soil after standing still at the filling site, and then rolling it with a vibrating roller until the compaction requirement is met, and the filling is completed.
2. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 1, characterized in that: The mass ratio of phosphogypsum, admixture and slaked lime in S1 is 1:0.1:0.02-0.
025.
3. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 2, characterized in that: The mass ratio of the clay in the S2 to the phosphogypsum in the S1 is 1:0.42-0.
48.
4. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 3, characterized in that: The moisture content of the improved soil obtained in S2 is controlled to be 1% to 2% above the optimum moisture content; the moisture content of the improved soil in S3 is controlled to be 1% to 2% above the optimum moisture content during rolling.
5. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 4, characterized in that: The test method for the optimal moisture content specifically includes: mixing clay, phosphogypsum, admixture and slaked lime in proportion to obtain improved soil, dividing the improved soil into no less than 5 groups by mass, adding different masses of water to each group of the improved soil to obtain no less than 5 groups of improved soil with a moisture content of 18% as a base point and an interval of 2%, performing compaction tests on the improved soils to obtain the dry density corresponding to each group of the improved soils, and drawing a curve chart of the relationship between moisture content and dry density. The moisture content at the peak point of the curve of the relationship between moisture content and dry density is the optimal moisture content of the improved soil; the mass ratio of the phosphogypsum, admixture and slaked lime is the same as the mass ratio of the phosphogypsum, admixture and slaked lime in S1, and the mass ratio of the clay and phosphogypsum is the same as the mass ratio of the clay in S2 and the phosphogypsum in S1.
6. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 5, characterized in that: After the S3 is filled, water is sprinkled on the surface of the compacted layer of the improved soil for 7 days for maintenance.
7. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 6, characterized in that: The calcium sulfate content in the phosphogypsum is not less than 75%; the pH of the phosphogypsum is 7-9.
8. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 7, characterized in that; The admixture comprises one or more of granulated blast furnace slag powder, fly ash and volcanic ash, and the volcanic ash activity index of the admixture at 28 days is not less than 75%.
9. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 8, characterized in that; The slaked lime is calcium slaked lime, and the grade of the slaked lime is HCL75 or above.
10. A roadbed filling method for transforming poor clay with industrial waste residues as claimed in claim 9, characterized in that; The clay includes one or more of swelling clay, high liquid limit clay and red clay.
Citation Information
Patent Citations
Improved formula of expansive soil and construction process using improved formula
CN105174906A
Cited By
Phosphogypsum composite modified expansive soil engineering filler as well as preparation method and application thereof
CN119859048A