Glass ceramic insulator preparation method, glass ceramic insulator and application
By preparing glass ceramic insulators and using specific raw material components and preparation processes, the problems of poor thermal shock resistance of ceramic insulators and self-explosion of glass insulators are solved, the force-thermal-optical-electrical properties of the insulators are improved, and the security of the power grid is enhanced. and stability.
Patent Information
- Application Number
- CN202410953105.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-08
AI Technical Summary
Ceramic insulators have poor thermal shock resistance and are prone to deterioration. Glass insulators have the risk of self-explosion, which affects the safety and stability of the power grid.
By preparing glass ceramic insulators, using specific raw material components (such as SiO2, Al2O3, MgO, ZnO, Y2O3, etc.) for ball milling and mixing, melting, nucleation and crystallization, combined with grinding and glue installation, we can prepare an insulator with excellent performance glass ceramic insulators.
It improves the force-thermal-optical-electrical properties of glass ceramic insulators, significantly reduces the risk of safety accidents caused by insulator failure, enhances the safety and reliability of insulators, and meets the needs of high-voltage power equipment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of insulators, and in particular to a preparation method of a glass ceramic insulator and the glass ceramic insulator and its application. Background Art
[0002] As an important component of power transmission lines, insulators are mainly used to support conductors and provide insulation. Therefore, they must have good mechanical and electrical properties. With the rapid development of electrified railways in my country, the demand for insulators in the railway network is increasing. The performance of insulators directly affects the normal power supply and driving safety of the railway. Once the quality of insulator products is damaged, it will seriously affect the safe and reliable operation of the railway power grid. In order to ensure the safety and stability of insulators, their performance requirements are receiving more and more attention.
[0003] At present, the insulators used in transmission lines are made of three materials: ceramic, glass and glass ceramic. Ceramic insulators are the most widely used in the insulator industry due to their high mechanical strength, stable chemical properties, good insulation performance and good corrosion resistance. However, ceramic insulators are brittle and have low reliability. During operation, they may experience problems such as reduced strength and interface breakdown, which greatly shortens the service life of ceramic insulators. At the same time, it will increase the maintenance cost of insulators and affect the normal operation of the power grid. Glass insulators are made of glass, which has high mechanical strength, is not prone to cracks on the surface, has high electrical breakdown strength, good insulation, excellent anti-aging performance, and good oil and arc resistance. The operation and maintenance costs are low, but the surface is prone to condensation of moisture, causing air dust to deposit and cause leakage. The self-explosion rate is high and it is not suitable for high voltage systems.
[0004] Glass ceramics, also known as microcrystalline glass or microcrystalline ceramics, are a solid phase material containing glass and polycrystalline obtained by controlled nucleation and crystallization of certain basic glasses of specific composition at a certain temperature. The performance of glass ceramics is mainly determined by the main crystal phase, which can be achieved by controlling nucleation, crystallization and selecting different mother glass components. Glass ceramics have the advantages of both glass and ceramics, and can solve the shortcomings of poor thermal shock resistance and easy degradation of the above-mentioned ceramic insulators and the shortcomings of glass insulators that are difficult to overcome and self-explosion. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to solve the problems of poor thermal shock resistance and self-explosion.
[0006] The present invention solves the above technical problems through the following technical means:
[0007] A first aspect of the present invention provides a method for preparing a glass ceramic insulator, comprising the following steps:
[0008] (1) mixing raw materials, a crystal nucleating agent and a dopant by ball milling according to weight percentage to obtain a mixed material; the raw materials include 10-15% MgO, 30-35% Al2O3 and 50-60% SiO2; the crystal nucleating agent is one or more of ZnO, ZrO2, TiO2 and P2O5; the weight percentage of the crystal nucleating agent in the raw materials is 2-8%; the dopant is one or more of Y2O3, La2O3 and CeO2; the weight percentage of the dopant in the raw materials is 0.01-0.6%;
[0009] (2) melting the mixed material, placing the melted mixed material in a preheated mold for annealing, and cooling it naturally to obtain a base glass;
[0010] (3) subjecting the base glass to a nucleation treatment and then a crystallization treatment, wherein the crystallization treatment is performed at a heating rate of 3 to 8°C / min, the temperature is raised to a crystallization temperature of 800 to 1150°C, the crystallization treatment is performed for 1 to 10 hours, and then annealing and cooling is performed to obtain a glass ceramic component of the insulator;
[0011] (4) The glass ceramic component is ground and polished and then glued to the metal component of the insulator to obtain a glass ceramic insulator.
[0012] Beneficial effects: The present invention successfully prepares glass ceramic insulators with excellent performance by adjusting the composition ratio of raw materials, crystal nucleating agents and dopants, and accurately controlling the temperature and time in the preparation process. The present invention adjusts the crystallization behavior of the material by adding a crystal nucleating agent, and improves the microstructure of the material by adding a dopant to improve the performance. The glass ceramic insulator prepared by the present invention solves the shortcomings of poor thermal shock resistance and easy self-explosion of the insulators caused by the inevitable defects of the materials themselves in the current ceramic insulators and glass insulators.
[0013] Preferably, the raw material further comprises 1-10% H3BO3 and 1-9% K2O.
[0014] Beneficial effects: The present invention promotes the precipitation of cordierite and improves material properties by adding boric acid and potassium oxide.
[0015] Preferably, the melting temperature is 1460-1680° C., and the melting time is 2-4 hours.
[0016] Preferably, the mold shape is one of a long rod type, a disc-shaped hanging type or a basin type.
[0017] Preferably, the preheating temperature is 600-900° C., the annealing temperature is 630-720° C., and the time is 0.5-3 h.
[0018] Preferably, the nucleation treatment is carried out at a heating rate of 3 to 8°C / min, with the temperature being raised to a nucleation temperature of 650 to 850°C, and the nucleation treatment is carried out for 2 to 6 hours.
[0019] Preferably, the crystallization temperature is 950-1050° C., and the crystallization treatment time is 2-6 hours.
[0020] Preferably, the binder is lead-antimony alloy.
[0021] The second aspect of the present invention provides a glass ceramic insulator obtained by the above preparation method.
[0022] The third aspect of the present invention provides the use of the glass ceramic insulators made by the above-mentioned preparation method in high-voltage power equipment.
[0023] The advantages of the present invention are: in view of the problems that ceramic insulators have poor thermal shock resistance and easy degradation and the potential for self-explosion of glass insulators, the glass-ceramic insulator of the present invention has higher safety and reliability, and its excellent mechanical-thermal-optical-electrical performance can significantly reduce the risk of safety accidents caused by insulator failures, which is of great significance for improving the stability of power grid operation. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0026] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0027] Example 1
[0028] This embodiment provides a long rod type glass ceramic insulator and a preparation method thereof, which specifically comprises the following steps:
[0029] (1) Weigh the components according to weight percentage as shown in the following table: Ball mill the components according to the table and mix them thoroughly to obtain a mixed material.
[0030] Components Weight Percent <![CDATA[SiO2]]> 55.4% <![CDATA[Al2O3]]> 30.5% MgO 14.1% <![CDATA[H3BO3]]> 8% <![CDATA[K2O]]> 3% ZnO 2.4% <![CDATA[Y2O3]]> 0.2%
[0031] (2) The mixed material is melted at 1680°C for 4 hours. When the solution is completely melted and uniform, it is quickly cast into a long rod insulator graphite mold preheated to 700°C for casting. The cast glass is placed in an annealing furnace at 650°C for annealing for 2 hours, cooled naturally to room temperature and taken out to obtain the basic glass.
[0032] (3) The base glass is placed in a high-temperature furnace and uniformly heated to a nucleation temperature of 850°C at a heating rate of 5°C / min, subjected to nucleation treatment for 4 hours, and then heated to a crystallization temperature of 1000°C at a rate of 5°C / min, subjected to crystallization treatment for 4 hours, and then taken out after annealing and cooling to obtain a glass ceramic component of the insulator.
[0033] (4) The glass ceramic component is then ground and polished and glued to the iron cap. The glue is a lead-antimony alloy. After cooling, a long rod glass ceramic insulator is obtained.
[0034] Example 2
[0035] This embodiment provides a long rod type glass ceramic insulator and a preparation method thereof, which specifically comprises the following steps:
[0036] (1) Weigh the components according to weight percentage as shown in the following table: Ball mill the components according to the table and mix them thoroughly to obtain a mixed material.
[0037] Components Weight Percent <![CDATA[SiO2]]> 51.8% <![CDATA[Al2O3]]> 34% MgO 14.2% <![CDATA[ZrO2]]> 4% <![CDATA[Y2O3]]> 0.2%
[0038] (2) The mixed material is melted at 1480°C for 4 hours. When the solution is completely melted and uniform, it is quickly cast into a long rod insulator graphite mold preheated to 650°C for casting. The cast glass is placed in an annealing furnace at 650°C for annealing for 1 hour, and naturally cooled to room temperature and taken out to obtain the basic glass.
[0039] (3) The base glass is placed in a high-temperature furnace and uniformly heated to a nucleation temperature of 650°C at a heating rate of 3°C / min, subjected to nucleation treatment for 5 hours, and then heated to a crystallization temperature of 950°C at a rate of 3°C / min, subjected to crystallization treatment for 6 hours, and then taken out after annealing and cooling to obtain a glass ceramic component of the insulator.
[0040] (4) The glass ceramic component is then ground and polished and glued to the iron cap. The glue is a low-melting-point lead-antimony alloy. After cooling, a long-rod glass ceramic insulator is obtained.
[0041] Example 3
[0042] This embodiment provides a disc-shaped suspension glass ceramic insulator and a preparation method thereof, which specifically includes the following steps:
[0043] (1) Weigh the components according to weight percentage as shown in the following table: Ball mill the components according to the table and mix them thoroughly to obtain a mixed material.
[0044] Components Weight Percent <![CDATA[SiO2]]> 57.9% <![CDATA[Al2O3]]> 30.1% MgO 12.0% <![CDATA[P2O5]]> 4% <![CDATA[La2O3]]> 0.3%
[0045] (2) The mixed material is melted at 1580°C for 3 hours. When the solution is completely melted and uniform, it is quickly cast into a long rod insulator graphite mold preheated to 800°C for casting. The cast glass is placed in an annealing furnace at 650°C for annealing for 2 hours, and naturally cooled to room temperature and taken out to obtain the basic glass.
[0046] (3) The base glass is placed in a high-temperature furnace and uniformly heated to a nucleation temperature of 850°C at a heating rate of 5°C / min, subjected to nucleation treatment for 4 hours, and then heated to a crystallization temperature of 950°C at a rate of 5°C / min, subjected to crystallization treatment for 4 hours, and then taken out after annealing and cooling to obtain a glass ceramic component of the insulator.
[0047] (4) The glass ceramic component is then ground and polished and glued to the iron cap. The glue is a low melting point lead-antimony alloy. After cooling, a disc-shaped suspension glass ceramic insulator is obtained.
[0048] Example 4
[0049] This embodiment provides a disc-shaped suspension glass ceramic insulator and a preparation method thereof, which specifically includes the following steps:
[0050] (1) Weigh the components according to weight percentage as shown in the following table: Ball mill the components according to the table and mix them thoroughly to obtain a mixed material.
[0051] Components Weight Percent <![CDATA[SiO2]]> 58.8% <![CDATA[Al2O3]]> 30.3% MgO 10.9% <![CDATA[H3BO3]]> 8% <![CDATA[K2O]]> 3% <![CDATA[ZrO2]]> 4% <![CDATA[CeO2]]> 0.2%
[0052] (2) The mixed material is melted at 1680°C for 4 hours. When the solution is completely melted and uniform, it is quickly cast into a long rod insulator graphite mold preheated to 700°C for casting. The cast glass is placed in an annealing furnace at 650°C for annealing for 2 hours, cooled naturally to room temperature and taken out to obtain the basic glass.
[0053] (3) The base glass is placed in a high-temperature furnace and uniformly heated to a nucleation temperature of 850°C at a heating rate of 5°C / min, subjected to nucleation treatment for 4 hours, and then heated to a crystallization temperature of 1025°C at a rate of 5°C / min, subjected to crystallization treatment for 2 hours, and then taken out after annealing and cooling to obtain a glass ceramic component of the insulator.
[0054] (4) The glass ceramic component is then ground and polished and glued to the iron cap. The glue is a low melting point lead-antimony alloy. After cooling, a disc-shaped suspension glass ceramic insulator is obtained.
[0055] Example 5
[0056] This embodiment provides a pot-type glass ceramic insulator and a preparation method thereof, which specifically includes the following steps:
[0057] (1) Weigh the components according to weight percentage as shown in the following table: Ball mill the components according to the table and mix them thoroughly to obtain a mixed material.
[0058] Components Weight Percent <![CDATA[SiO2]]> 51.8% <![CDATA[Al2O3]]> 34% MgO 14.2% <![CDATA[H3BO3]]> 8% <![CDATA[K2O]]> 3% <![CDATA[P2O5]]> 3% ZnO 5% <![CDATA[La2O3]]> 0.2% <![CDATA[CeO2]]> 0.2%
[0059] (2) The mixed material is melted at 1680°C for 4 hours. When the solution is completely melted and uniform, it is quickly cast into a long rod insulator graphite mold preheated to 700°C for casting. The cast glass is placed in an annealing furnace at 650°C for annealing for 2 hours, cooled naturally to room temperature and taken out to obtain the basic glass.
[0060] (3) The base glass is placed in a high-temperature furnace and uniformly heated to a nucleation temperature of 850°C at a heating rate of 5°C / min, subjected to nucleation treatment for 4 hours, and then heated to a crystallization temperature of 1050°C at a rate of 5°C / min, subjected to crystallization treatment for 4 hours, and then taken out after annealing and cooling to obtain a glass ceramic component of the insulator.
[0061] (4) The glass ceramic component is then ground and polished and glued to the iron cap. The glue is a low melting point lead-antimony alloy. After cooling, a basin-type glass ceramic insulator is obtained.
[0062] Comparative Example 1
[0063] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that the mass percentage of the raw material components in this comparative example is different from that in Example 1, namely SiO2: 40.1%, Al2O3: 34.1%, and MgO: 25.8%.
[0064] Comparative Example 2
[0065] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that in this comparative example, H3BO3 and K2O are added at 12% and 10% of the weight of the raw materials.
[0066] Comparative Example 3
[0067] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that the crystal nucleating agent in this comparative example is ZrO2 added at 15% of the weight of the raw material.
[0068] Comparative Example 4
[0069] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that the crystallization temperature in this comparative example is 1200° C. and the crystallization time is 12 h.
[0070] Comparative Example 5
[0071] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that in this comparative example 5, no dopant is added.
[0072] Comparative Example 6
[0073] The preparation method of the long rod type glass ceramic insulator in this comparative example is the same as that in Example 1, and specific reference is made to Example 1. The difference is that the dopant in this comparative example is Fe2O3 added at 0.3% of the weight of the raw material.
[0074] Performance Test:
[0075] The glass ceramic components prepared in Examples 1-5 and Comparative Examples 1-6 of the present invention were used as samples to perform performance tests according to GB / T8411.2 "Ceramic and Glass Insulating Materials Part 2: Test Methods". The test results are shown in Table 1 below:
[0076] Table 1 Performance test table
[0077] Light transmittance Vickers hardness Bending strength Coefficient of thermal expansion Dielectric constant Dielectric loss Example 1 88% 9.2GPa 188MPa <![CDATA[3.3×10 -6 / ℃]]> 5.9 <![CDATA[2.6×10 -3 ]]> Example 2 85% 9.3GPa 202MPa <![CDATA[3.5×10 -6 / ℃]]> 5.8 <![CDATA[2.5×10 -3 <!-- 5 -->]]> Example 3 87% 10.5GPa 180MPa <![CDATA[3.7×10 -6 / ℃]]> 6.0 <![CDATA[3.0×10 -3 ]]> Example 4 86% 8.9GPa 195MPa <![CDATA[3.6×10 -6 / ℃]]> 5.7 <![CDATA[2.6×10 -3 ]]> Example 5 90% 10.3GPa 205MPa <![CDATA[3.0×10 -6 / ℃]]> 5.4 <![CDATA[2.3×10 -3 ]]> Comparative Example 1 77% 7.3GPa 105MPa <![CDATA[5.5×10 -6 / ℃]]> 8.1 <![CDATA[6.8×10 -3 ]]> Comparative Example 2 69% 8.2GPa 128MPa <![CDATA[4.9×10 -6 / ℃]]> 8.8 <![CDATA[8.2×10 -3 ]]> Comparative Example 3 74% 7.3GPa 113MPa <![CDATA[5.6×10 -6 / ℃]]> 8.3 <![CDATA[7.0×10 -3 ]]> Comparative Example 4 77% 7.9GPa 92MPa <![CDATA[5.3×10 -6 / ℃]]> 9.1 <![CDATA[10.3×10 -3 ]]> Comparative Example 5 80% 8.3GPa 140MPa <![CDATA[4.7×10 -6 / ℃]]> 7.8 <![CDATA[5.1×10 -3 ]]> Comparative Example 6 65% 7.1 GPa 85MPa <![CDATA[5.9×10 -6 / ℃]]> 9.4 <![CDATA[17.4×10 -3 ]]>
[0078] The light transmittance in the table refers to the light transmittance when the thickness of the glass ceramic component is 2mm.
[0079] As shown in Table 1, the glass ceramic insulator prepared by the present invention has good mechanical-thermal-optical-electrical properties, can make up for the inherent defects of glass insulators and ceramic insulators, and meet the needs of ultra-high voltage power transmission and transformation projects. Comparative Examples 1 to 6 show that the raw material ratio, crystal nucleation agent, dopant, crystallization temperature and time can affect the performance of glass ceramic materials. Unreasonable raw material ratio, crystal nucleation agent, dopant and crystallization system will significantly reduce the material performance, so it is necessary to design a suitable material preparation plan.
[0080] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a glass ceramic insulator, characterized in that: The following steps are involved: (1) mixing raw materials, a crystal nucleating agent and a dopant by ball milling according to weight percentage to obtain a mixed material; the raw materials include 10-15% MgO, 30-35% Al2O3 and 50-60% SiO2; the crystal nucleating agent is one or more of ZnO, ZrO2, TiO2 and P2O5; the weight percentage of the crystal nucleating agent in the raw materials is 2-8%; the dopant is one or more of Y2O3, La2O3 and CeO2; the weight percentage of the dopant in the raw materials is 0.01-0.6%; (2) melting the mixed material, placing the melted mixed material in a preheated mold for annealing, and cooling it naturally to obtain a base glass; (3) subjecting the base glass to a nucleation treatment and then a crystallization treatment, wherein the crystallization treatment is performed at a heating rate of 3 to 8°C / min, the temperature is raised to a crystallization temperature of 800 to 1150°C, the crystallization treatment is performed for 1 to 10 hours, and then annealing and cooling is performed to obtain a glass ceramic component of the insulator; (4) The glass ceramic component is ground and polished and then glued to the metal component of the insulator to obtain a glass ceramic insulator.
2. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The raw material also includes 1-10% H3BO3 and 1-9% K2O.
3. The method for preparing a glass ceramic insulator according to claim 2, characterized in that: The melting temperature is 1460-1680° C., and the melting time is 2-4 hours.
4. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The mold shape is one of a long rod type, a disc-shaped hanging type or a basin type.
5. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The preheating temperature is 600-900° C., the annealing temperature is 630-720° C., and the time is 0.5-3 hours.
6. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The nucleation treatment is carried out at a heating rate of 3 to 8°C / min, the temperature is raised to a nucleation temperature of 650 to 850°C, and the nucleation treatment is carried out for 2 to 6 hours.
7. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The crystallization temperature is 950-1050° C., and the crystallization treatment time is 2-6 hours.
8. The method for preparing a glass ceramic insulator according to claim 1, characterized in that: The adhesive is a lead-antimony alloy.
9. A glass ceramic insulator is prepared according to the method for preparing a glass ceramic insulator as described in any one of claims 1 to 8.
10. Use of a glass ceramic insulator obtained by the method for preparing a glass ceramic insulator according to any one of claims 1 to 8 in high voltage power equipment.