Preparation method of hard carbon negative electrode material and hard carbon negative electrode plate for sodium ion battery

Through the preparation method of hybridizing transition metal sulfides and carbon materials, C-Co9S8/C material is formed, which solves the problem of insufficient cycle stability and rate performance of hard carbon anode materials in sodium-ion batteries, and achieves efficient cycle and rate performance of the battery. Increased capacity.

CN118748243AActive Publication Date: 2024-10-08HUINAN COUNTY JINYIJIA GREEN ENERGY BIOTECHNOLOGY CO LTD

Patent Information

Application Number
CN202410762271.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-08
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

The cycling stability and rate performance of existing hard carbon anode materials in sodium-ion batteries are insufficient, which limits their application scope and efficiency.

Method used

The preparation method of hybridizing transition metal sulfides and carbon materials is used to form a hybrid material of cobalt polysulfide and hard carbon through the steps of porous hard carbon materials, in-situ growth of zeolite imidazolate skeleton, sulfidation and carbon layer precursors, and A carbon layer is generated by polydopamine coating to form C-Co9S8/C material.

Benefits of technology

It improves the cycle stability and rate performance of sodium-ion batteries, optimizes battery electrode reaction kinetics, reduces electrochemical impedance, and significantly increases battery capacity and cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748243A_ABST
    Figure CN118748243A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a hard carbon negative electrode material for a sodium-ion battery, which comprises the following steps: preparing a porous hard carbon material, growing a zeolite imidazate skeleton on the surface of the porous hard carbon material in situ, vulcanizing, converting into a carbon layer precursor polydopamine-coated hard carbon material, and finally carbonizing, thereby obtaining the hard carbon negative electrode material for the sodium-ion battery. As a negative electrode material of a sodium ion battery, the volume expansion of the material is greatly relieved by a carbon layer formed by pyrolysis of dopamine hydrochloride, active sites of Co can be dispersed more uniformly, and more importantly, the cycling stability of the battery is greatly improved by the material wrapped by the carbon layer. The invention also discloses a preparation method of the hard carbon negative electrode plate for the sodium ion battery. According to the hard carbon negative electrode material for the sodium ion battery and the preparation method of the hard carbon negative electrode plate, the prepared negative electrode material improves the cycling stability and the rate capability of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a hard carbon negative electrode material for sodium ion batteries and a method for preparing a hard carbon negative electrode sheet. Background Art

[0002] Electrochemical energy storage has become a prominent technology for green energy utilization and has been widely studied and applied since the commercialization of lithium-ion batteries. However, the increase in the cost of lithium has made it urgent to find a new material to replace lithium-ion batteries. Sodium (Na) and lithium (Li) are elements of the same main group and have similar chemical properties to lithium. Therefore, sodium-ion batteries (SIBs) are considered to be the most excellent alternative to lithium-ion batteries. In addition, sodium is very abundant and widely distributed in seawater. It has a small charge-to-mass ratio, high stability, low solvation effect, and a wide redox electrochemical window, which is conducive to the construction of a stable battery system. With the increase in applications and the expansion of scope, sodium-ion battery technology is gradually finding ways to a richer and more sustainable system. The development of suitable electrode materials is at the core of this transformation.

[0003] At present, the negative electrode materials of sodium ion batteries are mainly divided into three categories according to their mechanism of storing sodium ions: carbon-based materials; transition metal oxides, sulfides, phosphides, etc.; alloy materials (Fe, Co, Ni, Mn, etc.). Among these three types of materials, materials based on conversion reactions have higher theoretical capacity and lower working potential, and are considered to be the most promising negative electrode materials.

[0004] Among them, carbon-based materials have the highest technical maturity and abundant resources, and are expected to be the first to achieve industrialization. Compared with the diameter of the sodium ion The large size of the anode leads to sluggish sodium ion reaction kinetics and significant electrode volume expansion, which limits the application of traditional graphite carbon in sodium ion batteries. Among carbon-based negative electrode materials, hard carbon (HC) is a feasible sodium ion embedded negative electrode material. It has a disordered, stacked microcrystalline structure with abundant sodium storage sites and a loose and suitable ion storage and transportation environment, which is not only conducive to the absorption of more Na, but also conducive to the embedding and de-embedding of Na. However, the development of materials with high rate and cycle stability is still a difficulty in current hard carbon negative electrode active materials. Summary of the invention

[0005] The purpose of the present invention is to provide a hard carbon negative electrode material for a sodium ion battery hybridized with a transition metal sulfide and a carbon material and a method for preparing a hard carbon negative electrode sheet. The prepared negative electrode material improves the cycle stability and rate performance of the battery.

[0006] In order to achieve the above object, the solution of the present invention is:

[0007] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0008] Step 1: Preparation of porous hard carbon material:

[0009] Buckwheat husk powder is first heated to 600-800°C at a heating rate of 3-5°C / min, and is kept warm for 2-3 hours under protective gas protection to obtain a carbon-based material, which is then soaked and washed with a KOH solution to obtain a porous hard carbon material, which is recorded as Buckwheat Carbon.

[0010] Step 2: In situ growth of zeolite imidazolate framework:

[0011] Then, the porous hard carbon material obtained in step 2 is ultrasonically dispersed in an ethanol solution of cobalt nitrate hexahydrate, and 2-methylimidazole is added to the solution after ultrasonication to in-situ generate a zeolite imidazolate skeleton on the surface of the porous hard carbon material to obtain a hard carbon material having a zeolite imidazolate skeleton, which is recorded as ZIF-67 Driven Carbon;

[0012] Step 3, vulcanization:

[0013] Then, the ZIF-67 Driven Carbon obtained in step 2 is mixed evenly with sulfur powder and placed in a tube furnace. The mixture is heated to 600-900° C. at a rate of 3-5° C. / min under protective gas protection and kept at this temperature for 2-3 hours. After cooling, a hybrid material of cobalt polysulfide and hard carbon is obtained, which is recorded as Co9S8 / C material.

[0014] Step 4: Generate carbon layer precursor:

[0015] Then, the Co9S8 / C material obtained in step 3 is ultrasonically dispersed in deionized water, and the solution is adjusted to weak alkalinity, and then dopamine hydrochloride is added, and a polymerization reaction occurs on the surface of the hybrid material under stirring to generate a polydopamine-coated material, which is stirred for 1 to 4 hours, centrifuged, and dried overnight at 60 to 80° C. to obtain a Co9S8 / C material coated with a carbon layer precursor;

[0016] Step 5: Carbonization:

[0017] Finally, the Co9S8 / C material obtained in step 4 is placed in a tubular furnace, and the temperature is raised to 600-900°C at 3-5°C / min under the protection of protective gas and kept for 2-3 hours to obtain the hard carbon negative electrode material for sodium ion battery, which is recorded as C-Co9S8 / C.

[0018] In step 1, the KOH solution immersion washing process is: disperse the carbon-based material obtained by pyrolysis in 100 mL of a KOH solution with a mass concentration of 10%, stir for 10 to 12 hours, centrifuge to obtain a precipitate, and then repeatedly wash the precipitate with dilute hydrochloric acid and anhydrous ethanol for multiple times, and dry it at 60 to 80°C overnight.

[0019] In step 2, the mass ratio of the porous hard carbon material to cobalt nitrate hexahydrate is 1-2:3, and the mass ratio of the 2-methylimidazole to cobalt nitrate hexahydrate is 1.5-2:1.

[0020] In step 3, the mass ratio of the ZIF-67 Driven Carbon to the sulfur powder is 3:1-3.

[0021] In step 4, the usage ratio of the Co9S8 / C material to deionized water is 0.5-1.5 g:50-100 mL.

[0022] In step 4, NaOH with a mass concentration of 33% is used to adjust the pH of the solution to 9.0.

[0023] In step 4, the mass ratio of dopamine hydrochloride to Co9S8 / C material is 0.5 to 1:4.

[0024] The protective gas is nitrogen.

[0025] A method for preparing a hard carbon negative electrode sheet for a sodium ion battery comprises the following steps: firstly preparing a slurry of the hard carbon negative electrode material for the sodium ion battery, a conductive agent and a binder according to a mass ratio of 8-9:0.5-1:0.5-1, then uniformly coating the prepared slurry on a copper foil, and vacuum drying the slurry at 80-100° C. for 10-12 hours to obtain the hard carbon negative electrode sheet for the sodium ion battery.

[0026] The conductive agent is carbon black, and the binder is polyvinylidene fluoride.

[0027] After adopting the above technical solution, the method for preparing a hard carbon negative electrode material for a sodium ion battery of the present invention has the following beneficial effects:

[0028] 1. First, the in-situ generated zeolite imidazolate skeleton will generate cobalt polysulfide after sulfidation, which will be embedded in the hard carbon material to obtain a hybrid material of cobalt polysulfide and hard carbon. The material hybridized with transition metal sulfide and carbon material is used as the negative electrode material for sodium ion batteries. After research, it is found that the hybridization of transition metal sulfide and carbon material can effectively prevent particle aggregation, limit volume expansion, etc., which can optimize the battery electrode reaction kinetics, increase the reaction rate, reduce the electrochemical impedance, increase the battery capacity, and more importantly, increase the battery cycle life.

[0029] 2. Secondly, polydopamine hydrochloride undergoes polymerization reaction on the surface of Co9S8 / C material to generate carbon layer precursor polydopamine coated material, which will form a carbon layer after pyrolysis and carbonization. The carbon layer formed by pyrolysis greatly alleviates the volume expansion of the electrode material, and can make the active site of Co nano-sized, dispersed more evenly and uniformly distributed. The wrapping of the carbon layer also makes the material have better cycle stability, and the larger specific surface area can fully contact with the electrolyte, thereby increasing the reaction rate.

[0030] 3. Finally, the test results of assembling the prepared hard carbon negative electrode sheet into a half-battery showed that the battery had good stability and low resistance during charging and discharging, and could significantly improve the battery capacity.

[0031] Therefore, the present invention provides a hard carbon negative electrode material for a sodium ion battery hybridized with a transition metal sulfide and a carbon material and a method for preparing a hard carbon negative electrode sheet. The prepared negative electrode material improves the cycle stability and rate performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 This is the SEM image of C-Co9S8 / C (3°C) prepared in Example 1;

[0033] Figure 2 This is the EDS (energy dispersive spectrum analysis) diagram of C-Co9S8 / C (3°C) prepared in Example 1;

[0034] Figure 3 TEM image of C-Co9S8 / C (3°C) prepared in Example 1;

[0035] Figure 4 This is the XRD pattern of C-Co9S8 / C (3°C) prepared in Example 1;

[0036] Figure 5 This is a comparison chart of the cycle performance of C-Co9S8 / C prepared in Examples 1 to 3;

[0037] Figure 6 This is the cycling performance diagram of C-Co9S8 / C (3°C) prepared in Example 1 at a current density of 10 A / g. DETAILED DESCRIPTION

[0038] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.

[0039] 1. Preparation of hard carbon negative electrode materials for sodium ion batteries

[0040] Example 1

[0041] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0042] Step 1: Preparation of porous hard carbon material:

[0043] Buckwheat husk powder was first sieved through a 200-mesh sieve, placed in a corundum porcelain boat and flattened, placed in a tubular furnace, introduced with nitrogen as a protective gas, heated to 600°C at a heating rate of 3°C / min, kept at this temperature for 2 hours for pyrolysis, and cooled to room temperature to obtain a carbon-based material;

[0044] The carbon-based material obtained by pyrolysis was dispersed in 100 mL of a 10% KOH solution, stirred for 12 hours, and centrifuged to obtain a precipitate. The precipitate was then washed repeatedly with dilute hydrochloric acid and anhydrous ethanol, and dried at 60° C. overnight to obtain a porous hard carbon material, which was recorded as Buckwheat Carbon.

[0045] Step 2: In situ growth of zeolite imidazolate framework:

[0046] Then, 0.5 g of the porous hard carbon material obtained in step 2 was ultrasonically dispersed in 100 mL of ethanol solution, and 1.46 g of cobalt nitrate hexahydrate was added. After ultrasonication for 20 minutes, 2.19 g of 2-methylimidazole was added to the ultrasonicated solution. After stirring at room temperature for 2 hours, the mixture was centrifuged and dried at 60° C. to obtain a hard carbon material having a zeolite imidazole ester skeleton, which was recorded as ZIF-67 Driven Carbon.

[0047] Step 3, vulcanization:

[0048] Then, the ZIF-67 Driven Carbon obtained in step 2 was mixed evenly with sulfur powder in a mass ratio of 3:1, placed in a tube furnace, nitrogen was introduced as a protective gas, the temperature was raised to 600°C at 3°C / min and kept for 2 hours, and after cooling, a hybrid material of cobalt polysulfide and hard carbon was obtained, which was recorded as Co9S8 / C material (3°C);

[0049] Step 4: Generate carbon layer precursor:

[0050] Then, 1.0 g of the Co9S8 / C material obtained in step 3 was ultrasonically dispersed in 100 mL of deionized water, and the pH of the solution was adjusted to 9.0 with 33% NaOH, and then 0.25 g of dopamine hydrochloride was added. After vigorous stirring for 15 min, the mixture was stirred for another hour, centrifuged, and dried at 60° C. overnight to obtain the Co9S8 / C material coated with the carbon layer precursor;

[0051] Step 5: Carbonization:

[0052] Finally, the Co9S8 / C material obtained in step 4 was placed in a corundum porcelain boat and flattened, placed in a tubular furnace, nitrogen was introduced as a protective gas, the temperature was raised to 600°C at 3°C / min, kept warm for 2 hours, and cooled to room temperature to obtain a hard carbon negative electrode material for sodium ion batteries, recorded as C-Co9S8 / C (3°C).

[0053] Example 2

[0054] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0055] Step 1: Preparation of porous hard carbon material:

[0056] Buckwheat husk powder was first sieved through a 200-mesh sieve, placed in a corundum porcelain boat and flattened, placed in a tubular furnace, introduced with nitrogen as a protective gas, heated to 800°C at a heating rate of 4°C / min, kept warm for 2.5 hours for pyrolysis, and cooled to room temperature to obtain a carbon-based material;

[0057] The carbon-based material obtained by pyrolysis was dispersed in 100 mL of a 10% KOH solution, stirred for 12 hours, and centrifuged to obtain a precipitate. The precipitate was then washed repeatedly with dilute hydrochloric acid and anhydrous ethanol, and dried at 80° C. overnight to obtain a porous hard carbon material, which was recorded as Buckwheat Carbon.

[0058] Step 2: In situ growth of zeolite imidazolate framework:

[0059] Then, 0.5 g of the porous hard carbon material obtained in step 2 was ultrasonically dispersed in 100 mL of ethanol solution, and 1.5 g of cobalt nitrate hexahydrate was added. After ultrasonication for 20 minutes, 3.0 g of 2-methylimidazole was added to the solution after ultrasonication. After stirring at room temperature for 2 hours, the solution was centrifuged and dried at 80° C. to obtain a hard carbon material having a zeolite imidazole ester skeleton, which was recorded as ZIF-67 Driven Carbon.

[0060] Step 3, vulcanization:

[0061] Then, the ZIF-67 Driven Carbon obtained in step 2 was mixed evenly with sulfur powder in a mass ratio of 3:2, placed in a tubular furnace, introduced with nitrogen as a protective gas, heated to 800°C at 4°C / min and kept warm for 2.5 hours, and after cooling, a hybrid material of cobalt polysulfide and hard carbon was obtained, which was recorded as Co9S8 / C material (4°C);

[0062] Step 4: Generate carbon layer precursor:

[0063] Then, 1.0 g of the Co9S8 / C material obtained in step 3 was ultrasonically dispersed in 100 mL of deionized water, and the pH of the solution was adjusted to 9.0 with 33% NaOH, and then 0.25 g of dopamine hydrochloride was added. After vigorous stirring for 15 min, the mixture was stirred for another 1.5 hours, centrifuged, and dried at 80°C overnight to obtain Co9S8 / C coated with a carbon layer precursor.

[0064] Step 5: Carbonization:

[0065] Finally, the carbon layer precursor obtained in step 4 was placed in a corundum porcelain boat and flattened, placed in a tubular furnace, nitrogen was introduced as a protective gas, the temperature was raised to 800°C at 4°C / min, kept warm for 2 hours, and cooled to room temperature to obtain a hard carbon negative electrode material for sodium ion batteries, recorded as C-Co9S8 / C (4°C).

[0066] Example 3

[0067] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:

[0068] Step 1: Preparation of porous hard carbon material:

[0069] Buckwheat husk powder was first sieved through a 200-mesh sieve, placed in a corundum porcelain boat and flattened, placed in a tubular furnace, introduced with nitrogen as a protective gas, heated to 800°C at a heating rate of 5°C / min, kept at this temperature for 2 hours for pyrolysis, and cooled to room temperature to obtain a carbon-based material;

[0070] The carbon-based material obtained by pyrolysis was dispersed in 100 mL of a 10% KOH solution, stirred for 10 hours, and centrifuged to obtain a precipitate. The precipitate was then washed repeatedly with dilute hydrochloric acid and anhydrous ethanol, and dried at 60° C. overnight to obtain a porous hard carbon material, which was recorded as Buckwheat Carbon.

[0071] Step 2: In situ growth of zeolite imidazolate framework:

[0072] Then, 0.5 g of the porous hard carbon material obtained in step 2 was ultrasonically dispersed in 100 mL of ethanol solution, and 1.46 g of cobalt nitrate hexahydrate was added. After ultrasonication for 20 minutes, 2.19 g of 2-methylimidazole was added to the ultrasonicated solution. After stirring at room temperature for 2 hours, the mixture was centrifuged and dried at 60° C. to obtain a hard carbon material having a zeolite imidazole ester skeleton, which was recorded as ZIF-67 Driven Carbon.

[0073] Step 3, vulcanization:

[0074] Then, the ZIF-67 Driven Carbon obtained in step 2 was mixed evenly with sulfur powder in a mass ratio of 1:1, placed in a tubular furnace, introduced with nitrogen as a protective gas, heated to 800°C at 5°C / min and kept at this temperature for 2 hours, and after cooling, a hybrid material of cobalt polysulfide and hard carbon was obtained, which was recorded as Co9S8 / C material (5°C);

[0075] Step 4: Generate carbon layer precursor:

[0076] Then, 0.5 g of the Co9S8 / C material obtained in step 3 was ultrasonically dispersed in 50 mL of deionized water, and the pH of the solution was adjusted to 9.0 with 33% NaOH, and then 0.125 g of dopamine hydrochloride was added. After vigorous stirring for 15 min, the mixture was stirred for another 1.5 hours, centrifuged, and dried at 60°C overnight to obtain the Co9S8 / C material coated with the carbon layer precursor;

[0077] Step 5: Carbonization:

[0078] Finally, the Co9S8 / C material obtained in step 4 was placed in a corundum porcelain boat and flattened, placed in a tubular furnace, nitrogen was introduced as a protective gas, the temperature was raised to 800°C at 5°C / min, kept warm for 2 hours, and cooled to room temperature to obtain a hard carbon negative electrode material for sodium ion batteries, recorded as C-Co9S8 / C (5°C).

[0079] Example 4

[0080] A method for preparing a hard carbon negative electrode sheet for a sodium ion battery comprises the following steps: firstly preparing a slurry of a hard carbon negative electrode material for a sodium ion battery, a conductive agent carbon black super P and a binder polyvinylidene fluoride in a mass ratio of 8:1:1, then uniformly coating the prepared slurry on a copper foil, and vacuum drying at 80°C for 12 hours to obtain the hard carbon negative electrode sheet for a sodium ion battery.

[0081] 2. Characterization of materials

[0082] Figure 1 This is the SEM image of the material C-Co9S8 / C (3°C) prepared in Example 1. The white particles in the image are Co9S8 with a particle size of about 1 μm. Figure 2 This is the EDS image of the material C-Co9S8 / C (3°C) prepared in Example 1. It can be seen from the image that the distribution of Co, S and N elements is relatively uniform.

[0083] Figure 3This is the TEM image of the material C-Co9S8 / C (3°C) prepared in Example 1. From the figure, it can be seen that the carbon layer boundary is very obvious. The whiter carbon layer (carbon layer) is obtained by thermal decomposition of polydopamine hydrochloride. The figure also shows the 200 crystal plane and 511 crystal plane of Co9S8, and the interlayer spacing is 0.2437nm and 0.1892nm respectively.

[0084] Figure 4 This is the XRD pattern of the material C-Co9S8 / C (3°C) prepared in Example 1. It can be seen from the figure that there are two obvious characteristic peaks at 2θ=29.888 and 2θ=52.186, which correspond to the peak values ​​of the standard PDF card No. 75-2023 of Co9S8 (Joint Committee on Powder Diffraction Standards, JCPDS card number).

[0085] 3. Performance testing

[0086] Figure 5 This is a comparison chart of the cycle performances of the hard carbon negative electrode materials prepared in Examples 1 to 3. It can be seen from the figure that the hard carbon negative electrode material corresponding to Example 1 has the highest reversible capacity.

[0087] Figure 6 The cycling performance of C-Co9S8 / C (3°C) prepared in Example 1 at a current density of 10 A / g. It can be seen from the figure that the material can still provide a reversible capacity of 186.15 mAh / g after 2000 cycles, and the capacity decay rate of each cycle is 0.07%, indicating that the hard carbon negative electrode material has good fast charging potential.

[0088] Therefore, the present invention provides a hard carbon negative electrode material for a sodium ion battery hybridized with a transition metal sulfide and a carbon material and a method for preparing a hard carbon negative electrode sheet. The prepared hard carbon negative electrode material improves the cycle stability and rate performance of the battery.

[0089] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.

Claims

1. A method for preparing a hard carbon negative electrode material for a sodium ion battery, characterized in that: The following steps are involved: Step 1: Preparation of porous hard carbon material: Buckwheat husk powder is first heated to 600-800°C at a heating rate of 3-5°C / min, and is kept warm for 2-3 hours under protective gas protection to obtain a carbon-based material, and then soaked and washed with a KOH solution to obtain a porous hard carbon material; Step 2: In situ growth of zeolite imidazolate framework: Then, the porous hard carbon material obtained in step 2 is ultrasonically dispersed in an ethanol solution of cobalt nitrate hexahydrate, and 2-methylimidazole is added to the solution after ultrasonication to in-situ generate a zeolite imidazolate skeleton on the surface of the porous hard carbon material to obtain a hard carbon material having a zeolite imidazolate skeleton; Step 3, vulcanization: Then, the hard carbon material having a zeolite imidazolate skeleton obtained in step 2 is mixed evenly with sulfur powder and placed in a tubular furnace, heated to 600-900° C. at 3-5° C. / min under protective gas protection and kept warm for 2-3 hours, and then cooled to obtain a hybrid material of cobalt polysulfide and hard carbon; Step 4: Generate carbon layer precursor: Then, the hybrid material of cobalt polysulfide and hard carbon obtained in step 3 is ultrasonically dispersed in deionized water, and the solution is adjusted to weak alkalinity, and then dopamine hydrochloride is added, and a polymerization reaction occurs on the surface of the hybrid material under stirring to generate a polydopamine-coated material, and then the material is stirred for 1 to 4 hours, centrifuged, and dried overnight at 60 to 80° C. to obtain a hybrid material of cobalt polysulfide and hard carbon coated with a carbon layer precursor; Step 5: Carbonization: Finally, the hybrid material of cobalt polysulfide and hard carbon obtained in step 4 is placed in a tubular furnace, and the temperature is raised to 600-900° C. at 3-5° C. / min under the protection of protective gas and kept at this temperature for 2-3 hours to obtain the hard carbon negative electrode material for sodium ion battery.

2. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 1, the KOH solution immersion washing process is: disperse the carbon-based material obtained by pyrolysis in 100 mL of a KOH solution with a mass concentration of 10%, stir for 10 to 12 hours, centrifuge to obtain a precipitate, and then repeatedly wash the precipitate with dilute hydrochloric acid and anhydrous ethanol for multiple times, and dry it at 60 to 80°C overnight.

3. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 2, the mass ratio of the porous hard carbon material to cobalt nitrate hexahydrate is 1-2:3, and the mass ratio of the 2-methylimidazole to cobalt nitrate hexahydrate is 1.5-2:

1.

4. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 3, the mass ratio of the hard carbon material having a zeolite imidazolate skeleton to the sulfur powder is 3:1-3.

5. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 4, the ratio of the hybrid material of cobalt polysulfide and hard carbon to deionized water is 0.5-1.5 g: 50-100 mL.

6. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 4, NaOH with a mass concentration of 33% is used to adjust the pH of the solution to 9.

0.

7. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: In step 4, the mass ratio of the hybrid material of dopamine hydrochloride and cobalt polysulfide to hard carbon is 0.5 to 1:

4.

8. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: The protective gas is nitrogen.

9. A method for preparing a hard carbon negative electrode sheet for a sodium ion battery, characterized in that: The following steps are involved: First, a hard carbon negative electrode material for a sodium ion battery, a conductive agent and a binder are prepared into a slurry in a mass ratio of 8 to 9: 0.5 to 1: 0.5 to 1, and then the prepared slurry is evenly coated on a copper foil, and after vacuum drying at 80 to 100° C. for 10 to 12 hours, the hard carbon negative electrode sheet for a sodium ion battery is obtained, wherein the hard carbon negative electrode material for a sodium ion battery is prepared by the preparation method of a hard carbon negative electrode material for a sodium ion battery as claimed in claim 1.

10. The method for preparing a hard carbon negative electrode sheet for a sodium ion battery according to claim 9, characterized in that: The conductive agent is carbon black, and the binder is polyvinylidene fluoride.

Citation Information

Patent Citations

  • Efficient hard carbon material and preparation method and application of efficient hard carbon material

    CN108682815A

  • Negative electrode composite material and preparation method and application thereof

    CN117790729A

  • Sodium-ion battery composite negative electrode material and preparation method thereof, negative electrode plate and secondary battery

    CN117913256A

  • Method for preparing composite negative electrode material for lithium ion battery

    US20190036108A1

Cited By

  • Modified filter medium, preparation method thereof and multi-medium filter

    CN119140063A