Preparation method and application of metal coordination crosslinking anti-plasticizing hollow fiber membrane

The preparation method of metal coordination cross-linked anti-plasticization hollow fiber membranes solves the problem of plasticization of hollow fiber membranes under high pressure, achieves gas separation performance stability under high CO2 content and high pressure conditions, and is suitable for a variety of gases Separate applications.

CN118751079AActive Publication Date: 2024-10-11GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411149844.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-10-11
Estimated Expiration
2044-08-21

AI Technical Summary

Technical Problem

Existing hollow fiber membranes are easily plasticized by gases such as carbon dioxide under high pressure conditions, resulting in reduced separation performance, and there is insufficient research on anti-plasticization properties.

Method used

The preparation method of metal coordination cross-linked anti-plasticization hollow fiber membranes is adopted. Through the dry-jet-wet spinning spinning process, polymers with specific structures are used to cross-link with non-solvent metal salts to form a membrane with excellent anti-plasticization properties. Hollow fiber membrane.

Benefits of technology

The prepared hollow fiber membrane shows strong resistance to carbon dioxide plasticization under high pressure, maintains gas selectivity, and is suitable for applications such as natural gas purification and carbon dioxide capture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751079A_ABST
    Figure CN118751079A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of gas separation membranes, and provides a preparation method of a metal coordination crosslinking anti-plasticizing hollow fiber membrane, and the preparation method comprises the following steps: (1) synthesizing a polyimide polymer from a diamine monomer containing carboxylic acid and a dianhydride monomer according to a certain proportion through a chemical imine method; (2) preparing a spinning solution from the polymer, an organic solvent, metal salt and a non-solvent according to a certain proportion; and (3) spinning the prepared spinning solution into a membrane according to certain conditions, soaking the membrane in pure water for a certain period of time, and cleaning the membrane with methanol and n-hexane for several times to remove the solvent. And (4) drying the cleaned hollow fiber membrane, and packaging into a membrane assembly for gas separation test. The obtained hollow fiber membrane can be applied to natural gas deacidification gas and natural gas helium extraction, and has excellent plasticizing resistance and gas separation performance. The method has the advantages that the process is stable, the operation is simple, and the gas separation and anti-plasticizing properties of the membrane are excellent. The research, development and preparation thinking of the anti-plasticizing hollow fiber membrane for gas separation is enriched, and the prepared anti-plasticizing hollow fiber membrane material has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas separation membranes, and in particular to a method for preparing a metal coordinated cross-linked plasticization-resistant hollow fiber membrane. Background Art

[0002] Gas separation is widely used in chemical production, energy resources, environmental protection and other fields, such as natural gas decarbonization, carbon dioxide capture, hydrogen separation and purification, oxygen and nitrogen separation, natural gas helium extraction and olefin and alkane separation. Compared with cryogenic distillation and pressure swing adsorption, membrane separation technology has the advantages of high separation efficiency, low energy consumption, small environmental footprint, and low equipment investment cost. It has been rapidly developed in the field of gas separation. Among them, polymer membranes have the advantages of low cost and high processability. They can be designed into different forms, especially asymmetric hollow fiber membranes, which are favored in industrial applications due to their high spatial specific surface area. However, the commercial hollow fiber membranes currently available for gas separation are easily plasticized by gases such as carbon dioxide under high-pressure operating conditions, resulting in reduced separation performance. For this reason, it is of great significance to develop a new structure of anti-plasticization hollow fiber membranes.

[0003] The patent (CN116272441B) discloses a gas separation membrane material for helium extraction from natural gas with an anti-plasticization effect, which uses two diamine monomers and a dianhydride monomer to synthesize a polyimide polymer, and then prepares a gas separation membrane. At a certain temperature, the carboxyl groups on the polymer molecular chain can be removed by heat treatment, so that a two-way ester exchange cross-linking reaction occurs to form a stable cross-linked structure. However, this patent is limited to the preparation of flat membranes and does not involve the preparation process of hollow fiber membranes. In addition, the cross-linking method of heat treatment easily reduces the gas permeability coefficient of the hollow fiber membrane.

[0004] The patent (CN117101428A) discloses a process for preparing chlorinated polyvinyl chloride hollow fiber membranes. The hollow fiber membranes prepared by the patent have good toughness, large filtration flux, high strength of the inner and outer skin layers of the membrane material, and good durability. However, the hollow fiber membrane material prepared by the patent is mainly used for liquid-solid separation and liquid-liquid separation, and does not involve gas separation. The raw material components used are mainly chlorinated polyvinyl chloride and styrene-ethylene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, and styrene-butylene-propylene-styrene block copolymers, and do not involve research on anti-plasticization performance.

[0005] The patent (CN116943460 B) discloses a method for preparing a hollow fiber composite membrane based on rare earth coordination, which is to immerse the purchased hollow fiber membrane in an organic solvent, generate amino groups on the surface of the hollow fiber membrane under ultraviolet light radiation, and then immerse it in a mixed solution of metal salts to prepare a hollow fiber composite membrane with rare earth coordination. However, the patent only involves the preparation of a hollow fiber composite membrane with rare earth coordination, and does not study the anti-plasticization performance of the hollow fiber membrane.

[0006] The patent (CN202310158174.X) discloses a method for preparing a high-strength anti-plasticization gas separation membrane. The polymer of the hollow fiber membrane is polymerized by 6FDA (hexafluorodianhydride) and DABA (3,5-diaminobenzoic acid), BPDA (3,3',4,4'-biphenyltetracarboxylic dianhydride), PMDA (1,2,4,5-pyromellitic dianhydride) and other diamines, which can reduce the fluidity of the polymer chain and improve the anti-plasticization performance and mechanical strength of the polymer. The hollow fiber membrane made by spinning the polyimide has the advantages of high strength, anti-plasticization and good thermal stability in the gas separation process. The hollow fiber membrane can maintain good CO while improving the permeability. 2 / N 2 and CO 2 / CH 4 However, the preparation method of this patent is complicated and the anti-plasticization performance needs to be strengthened.

[0007] The invention provides a metal coordinated hollow fiber membrane material. The hollow fiber membrane has high gas separation selectivity and excellent anti-plasticization effect under high pressure. Summary of the invention

[0008] In view of this, the present invention provides a method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane. The method is simple and easy to implement. The prepared hollow fiber membrane has a strong ability to resist plasticization by carbon dioxide, which is of great significance for maintaining the gas selectivity of the hollow fiber membrane in a real environment.

[0009] The metal coordinated cross-linked anti-plasticization hollow fiber membrane of the present invention is mainly characterized in that:

[0010] 1. The polymer used in the metal coordination cross-linked anti-plasticization hollow fiber membrane has a structure of formula (I):

[0011]

[0012] In formula (I), R 1 is a dianhydride monomer selected from R a , R b , R c Any one of the groups; R 2is a diamine monomer not containing a carboxyl group, which is selected from R d , R e , R f , R g Any one of the groups; R 3 is a diamine monomer containing a carboxyl group, selected from R h , R i , R j Any one of the groups.

[0013]

[0014] 2. The non-solvent metal salts used in the metal coordination cross-linking anti-plasticization hollow fiber membrane include but are not limited to ferric chloride, aluminum chloride, lanthanum chloride, europium chloride, cerium chloride and yttrium chloride.

[0015] 3. The method for preparing the metal coordinated cross-linked anti-plasticization hollow fiber membrane adopts a dry-jet-wet spinning process.

[0016] One of the purposes of the present invention is to provide a method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane, the technical scheme adopted is:

[0017] (1) mixing a polymer, a solvent, a metal salt and a non-solvent in a stirred kettle according to a certain component ratio and stirring until they are completely dissolved to obtain a spinning solution, and vacuum degassing the spinning solution to maintain the vacuum degree in the kettle at 10-50 kPa; after the degassing is complete, nitrogen is introduced into the kettle until the pressure reaches 0.4-0.8 MPa;

[0018] (2) mixing the solvent and deionized water in a certain proportion to evenly prepare the core liquid, and vacuuming and degassing the liquid for later use;

[0019] (3) The prepared spinning solution and core solution are squeezed into a spinneret of a specific size through a spinning pump at a certain flow rate, and are simultaneously squeezed out of the spinneret, pass through a certain air gap height under the pull of gravity and a guide wheel, and then enter a coagulation bath to solidify into a hollow fiber membrane;

[0020] (4) The initially formed hollow fiber membrane is pulled up by the guide wheel at a certain speed and collected on the collection wheel;

[0021] (5) The collected hollow fiber membranes are post-treated under certain conditions, first soaked in pure water for several days, the pure water is changed every once in a while, and then washed several times with non-solvent A and non-solvent B, and the non-solvent is changed every once in a while;

[0022] (6) The treated hollow fiber membrane is placed in a vacuum drying oven and dried at a specified temperature for a certain period of time.

[0023] In the above step (1), the solvent includes but is not limited to N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc) and tetrahydrofuran (THF), and the non-solvent includes but is not limited to water, ethanol, ethyl acetate and acetic acid.

[0024] In the above step (1), the proportion of the spinning solution components is as follows: the polymer component content is 20-30wt%, the solvent component content is 40-60wt%, the non-solvent component content is 10-20wt%, and the metal salt component content is 2-5wt%;

[0025] Preferably, the proportions of the polymer, solvent, non-solvent and metal salt in the spinning solution of step (1) are 27wt%, 55wt%, 15wt% and 3wt% respectively;

[0026] In the above step (2), the solvent content of the core liquid component is 10-30wt%; the solvent is selected from one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and tetrahydrofuran;

[0027] Preferably, the volume percentage content of the solvent in the core liquid in step (2) is 80%;

[0028] In the above step (3), the feed liquid flow rate is 10-15 ml / min, the core liquid flow rate is 5-10 ml / min; the outer diameter of the spray core is 0.5-1.0 mm, and the inner diameter is 0.3-0.8 mm; the air gap height is 5-15 cm;

[0029] Preferably, the feed liquid flow rate in step (3) is 10 ml / min, the core liquid flow rate is 5 ml / min; the air gap height is 7 cm;

[0030] In the above step (4), the stretching speed is 15-40 m / min;

[0031] Preferably, the stretching speed in step (4) is 30 m / min;

[0032] The post-treatment conditions of the above step (5) are as follows: the soaking time in pure water is 3-5 days, and the water is changed every 6-12 hours; the non-solvent A and the non-solvent B are washed 3-5 times each, and the water is changed every 30-60 minutes; the non-solvent A is selected from one of methanol, ethanol and isopropanol; the non-solvent B is selected from one of n-hexane and n-heptane;

[0033] In the above step (6), the drying temperature is 50-100° C. and the drying time is 12-18 hours;

[0034] Preferably, the drying temperature in step (6) is 100° C. and the drying time is 15 hours.

[0035] The second purpose of the present application is to provide a metal coordinated cross-linked anti-plasticization hollow fiber membrane product, characterized in that the metal coordinated cross-linked anti-plasticization hollow fiber membrane synthesized by the present invention has good gas separation performance.

[0036] The third purpose of the present application is to provide a use of a metal coordination cross-linked anti-plasticization hollow fiber membrane for gas separation, characterized in that the metal coordination cross-linked anti-plasticization hollow fiber membrane prepared according to the method of the present invention can be used for natural gas purification, carbon dioxide capture, hydrogen separation and purification, air separation, natural gas helium extraction, gas dehumidification and olefin alkane separation. Compared with the prior art, the hollow fiber membrane prepared by the present invention has a stronger anti-plasticization ability, and its performance is better in high CO 2 The gas separation performance can remain stable under the conditions of high content and high pressure inlet gas.

[0037] Example 1

[0038] A metal coordination cross-linked anti-plasticization hollow fiber membrane is prepared by the following method:

[0039] (1). Under nitrogen protection, in a 30L reactor equipped with a mechanical stirrer, first add DABA (199.5g), TFMB (70.0g) and MPDA (307.3g), then add anhydrous NMP (10L), after the diamine monomer is completely dissolved, cool the temperature in the reactor to 5°C, then add 6FDA (1942g) for polymerization reaction, and the reaction is completed after 8 hours to obtain the corresponding polyamide acid solution. Then, add 2113ml pyridine and 2479mL acetic anhydride for imide reaction, and react at 20°C for 24 hours to obtain a polyimide solution; the obtained polyimide solution is precipitated in pure water, and the precipitated polyimide material is poured into an aqueous solution containing 50% ethanol and stirred at the same time. After the completely precipitated polymer is washed three times with 50% ethanol solution, it is vacuum dried at 100°C for 12 hours to obtain a dry polyimide polymer.

[0040] (2) Take 400 g of the polyimide polymer (PI) obtained in step (1) and dissolve it in anhydrous NMP (667 g), place it in a spinning kettle, then add 222 g of anhydrous ethanol, 148 g of THF and 44.5 g of cerium chloride, stir for 48 hours to obtain the spinning solution, vacuum degassing and let it stand for 12 hours, and fill the kettle with nitrogen until the pressure reaches 0.4 MPa.

[0041] (3) The polyimide spinning solution obtained in step (2) is spun, and the spinning schematic diagram is as follows Figure 1As shown. First, the spinning liquid reaches the spinning pump through the pipeline under the nitrogen pressure of 0.4MPa in the kettle. The spinning pump squeezes the spinning liquid and the core liquid out of the nozzle at a certain feeding speed. After a certain gas height, it solidifies into a metal coordination cross-linked hollow fiber membrane in the coagulation bath. Among them, the spinning liquid discharge speed is 10mL / min, the core liquid discharge speed is 5mL / min, and the core liquid composition is 80wt% NMP and 20wt% H 2 O composition, the spinneret temperature is controlled at 50 ° C, and the spinneret is 7 cm above the coagulation bath to ensure the formation of the cortex of the hollow fiber membrane. Finally, the hollow fiber membrane is basically solidified in the coagulation bath, and the temperature of the coagulation bath is controlled at 20 ° C; the hollow fiber membrane is finally collected on the winding wheel, and the wheel winding speed is controlled at 30 m / min.

[0042] (4) Completely immerse the hollow fiber membrane obtained in step (3) in pure water, and change the water every 12 hours. After soaking for 72 hours, clean it, first soak it in methanol for 30 minutes, then rinse it with n-hexane for 30 minutes, and repeat the above operation 3 times. The cleaned hollow fiber membrane is placed in a vacuum drying oven and vacuumed at 100°C for 15 hours. The dried hollow fiber composite membrane packaging assembly is tested.

[0043] The cross-sectional morphology of the metal coordinated cross-linked anti-plasticization hollow fiber membrane prepared in this embodiment was analyzed by EDS energy spectrum scanning. Figure 2 As shown in the EDS energy spectrum scanning results, it can be seen that the metal Ce element is evenly distributed in the cross section of the hollow fiber membrane, and there is no agglomeration phenomenon in the cross section of the membrane, which indicates that the rare earth Ce has not been leached out of the membrane after 72 hours of pure water immersion, and the metal Ce exists in the hollow fiber membrane.

[0044] Comparative Example 1

[0045] An uncoordinated cross-linked hollow fiber membrane, the preparation conditions and method are similar to those of Example 1. The difference between the uncoordinated cross-linked hollow fiber membrane and Example 1 is that the cerium chloride of the inorganic salt in the spinning solution is replaced by lithium nitrate, and the other preparation conditions and methods are the same as those of Example 1.

[0046] The uncoordinated cross-linked hollow fiber membrane prepared in this comparative example was subjected to infrared spectroscopy analysis and gas performance test, and compared with the metal coordinated cross-linked anti-plasticization hollow fiber membrane prepared in Example 1. Figure 3 As shown, at wave number 1650cm -1 At the point, the hollow fiber membrane prepared in Control Example 1 has a characteristic peak of carboxyl groups, while the metal coordination cross-linking anti-plasticization hollow fiber membrane prepared in Example has no such peak, which indicates that the carboxyl groups on the hollow fiber membrane of Example undergo a coordination cross-linking reaction with the metal Ce ions.

[0047] The hollow fiber membranes prepared in Example 1 and Control Example 1 were subjected to gas performance tests. The test results are shown in Table 1. Compared with the uncoordinated cross-linked hollow fiber membrane, the gas permeability of the metal coordinated cross-linked anti-plasticization hollow fiber membrane decreased slightly, but the selectivity was improved.

[0048] Using He / CO 2 / CH 4 The anti-plasticization performance of two hollow fiber membranes was tested by mixing gas (0.3:49.4:50.3, v / v / v). The test results are as follows Figure 4 The results show that when the feed pressure of carbon dioxide reaches 400PSIA, the He / CH 4 The selectivity decreased significantly, while the metal coordination cross-linked anti-plasticization hollow fiber membrane He / CH 4 The selectivity remained basically unchanged, indicating that the metal-crosslinked hollow fiber membrane had a certain anti-plasticity ability.

[0049] Example 2

[0050] (1) A metal coordinated cross-linked anti-plasticization hollow fiber membrane is prepared by the method of Example 1, and the spinning parameters are set as follows: PI / NMP / THF / EtOH / LiNO 3 (27 / 45 / 10 / 15 / 3, wt%) is the mass ratio of feed liquid, H 2 Spinning was carried out under the conditions of O / NMP (80 / 20, v / v%) as the core liquid formula, pure water (20°C) as the coagulation bath, a fixed liquid flow rate of 10 ml / min, an air gap height of 7 cm, a spinneret temperature of 50°C and a stretching speed of 30 m / min.

[0051] (2) The difference from Example 1 is that a different core liquid flow rate of 10 ml / min is used for spinning.

[0052] The morphology of the metal coordinated cross-linked anti-plasticization hollow fiber membranes prepared in this embodiment and in Example 1 was scanned by electron microscope, and the relevant SEM electron microscope images are shown in the attached drawings. Figure 5 As shown in the figure, the change of the core liquid flow rate (feed liquid / core liquid flow rate ratio) has a great influence on the morphology of the hollow fiber. When the core liquid flow rate is 5 ml / min, the thickness of the hollow fiber membrane wall is 100 microns. When the core liquid flow rate increases to 10 ml / min, the thickness of the hollow fiber membrane wall decreases to 50 microns.

[0053] Example 3

[0054] (1) A metal coordinated cross-linked anti-plasticization hollow fiber membrane is prepared by the method of Example 1, and the spinning parameters are set as follows: PI / NMP / THF / EtOH / LiNO3 (27 / 45 / 10 / 15 / 3, wt%) is the mass ratio of feed liquid, H 2 Spinning was carried out under the conditions of O / NMP (80 / 20, v / v%) as the core liquid formula, pure water (20°C) as the coagulation bath, a fixed liquid flow rate of 10 ml / min, a core liquid flow rate of 5 ml / min, a spinneret temperature of 50°C and a stretching speed of 30 m / min.

[0055] (2) The difference from Example 1 is that different air gap heights are used for spinning, namely 1 cm and 14 cm, numbered 3-1 and 3-2 respectively.

[0056] The metal coordination cross-linked anti-plasticization hollow fiber membrane prepared in this embodiment was subjected to pure gas test, and the relevant results are shown in Table 1. As can be seen from the table, with the increase of the air gap height, the gas flux of the prepared hollow fiber membrane will decrease. When the air gap height is 1 cm, the selectivity of the prepared hollow fiber membrane is the lowest, among which He / CH 4 The selectivity is 19.6, which is obviously defective; when the air gap height is 7 cm (Example 1), the gas separation performance of the metal coordination cross-linked anti-plasticization hollow fiber membrane is the best, He / CH 4 and CO 2 / CH 4 The selectivities reached 257 and 49 respectively.

[0057] Example 4

[0058] (1) A metal coordinated cross-linked anti-plasticization hollow fiber membrane is prepared by the method of Example 1, and the spinning parameters are set as follows: 2 Spinning was carried out under the conditions of O / NMP (80 / 20, v / v%) as the core liquid formula, pure water (20°C) as the coagulation bath, a fixed liquid flow rate of 10 ml / min, a core liquid flow rate of 5 ml / min, a spinneret temperature of 50°C and a stretching speed of 30 m / min.

[0059] (2) The difference from Example 1 is that a different spinning solution formula is used for spinning, and the spinning solution formula composition is PI / NMP / THF / EtOH / LiNO 3 (22 / 45 / 10 / 20 / 3, wt%).

[0060] The metal coordination cross-linked anti-plasticization hollow fiber membrane prepared in this embodiment was subjected to pure gas testing, and the relevant results are shown in Table 1. The results show that as the polymer content of the spinning solution increases, the gas permeability decreases; when the solid content of the spinning solution is 22wt%, its gas selectivity is significantly low, because the viscosity of the spinning solution will also decrease due to the low solid content, resulting in defects in the spun hollow fiber membrane.

[0061] Example 5

[0062] (1) A metal coordinated cross-linked anti-plasticization hollow fiber membrane is prepared by the method of Example 1, and the spinning parameters are set as follows: PI / NMP / THF / EtOH / LiNO 3 (27 / 45 / 10 / 15 / 3, wt%) is the mass ratio of feed liquid, H 2 The spinning was carried out under the conditions of O / NMP (80 / 20, v / v%) as the core liquid formula, pure water (20°C) as the coagulation bath, a fixed liquid flow rate of 10 ml / min, a core liquid flow rate of 5 ml / min, and a spinneret temperature of 50°C.

[0063] (2) The difference from Example 1 is that different stretching speeds are used for spinning the core liquid components, namely 22.5 m / min and 15 m / min, numbered 5-1 and 5-2 respectively.

[0064] The tensile properties of the metal coordinated cross-linked anti-plasticization hollow fiber membrane prepared in this embodiment were tested, and the relevant results are shown in Table 2. As can be seen from the table, the hollow fiber prepared at a higher tensile speed has a higher tensile stress and elastic modulus, and the spun hollow fiber is more compact and has a lower porosity.

[0065] Table 1 Gas properties corresponding to different air gap heights

[0066]

[0067] Table 2 Effect of different stretching speeds on tensile properties

[0068] BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 This is a diagram of the hollow fiber membrane spinning process of Example 1;

[0070] Figure 2 This is the EDS spectrum of the cross section of the hollow fiber membrane in Example 1;

[0071] Figure 3 The infrared spectra of the hollow fiber membranes prepared in Example and Comparative Example 1 are shown;

[0072] Figure 4 The cross-sectional morphology scanning electron microscope images of the hollow fiber membranes prepared in Example and Comparative Example 1;

[0073] Figure 5 The hollow fiber membrane He / CO prepared in Example 1 and Comparative Example 1 2 / CH 4 (0.3:49.4:50.3,v / v / v) Mixed gas test results chart.

Claims

1. A method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane, characterized in that: The polyimide polymer used in the metal coordination cross-linked anti-plasticization hollow fiber membrane is polymerized from diamine monomers and dianhydride monomers by a chemical imide method, and has the following structural formula: In formula (I), R1 is a dianhydride monomer selected from R a , R b , R c Any one or more combinations of groups; R2 is a diamine monomer that does not contain a carboxylic acid group, which is selected from R d , R e , R f , R g Any one or more combinations of groups; R3 is a diamine monomer containing a carboxylic acid group, selected from R h , R i , R j Any one of the groups kind.

2. The method for preparing the metal coordinated cross-linked anti-plasticization hollow fiber membrane according to claim 1, characterized in that: The ratio of the diamine monomer containing a carboxylic acid group in all diamine monomers, ie, n / (m+n), is above 50%.

3. A method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane, characterized in that: The metal salts used in the metal coordination cross-linked anti-plasticization hollow fiber membrane include but are not limited to ferric chloride, aluminum chloride, lanthanum chloride, europium chloride, cerium chloride and yttrium chloride.

4. A method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane, characterized in that: The preparation method adopts a dry-jet-wet spinning process.

5. A process for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane according to claim 4, characterized in that: The preparation method comprises the following steps: (1) mixing a polymer, a solvent, a metal salt and a non-solvent in a stirred tank according to a certain component ratio and stirring until they are completely dissolved to obtain a spinning solution, vacuuming and degassing the spinning solution to maintain a vacuum degree in the tank at 10-50 kPa, and introducing nitrogen into the tank after the degassing is complete until the pressure reaches 0.4-0.8 MPa; (2) mixing the solvent and deionized water in a certain ratio to uniformly prepare the core liquid, and vacuuming and degassing the core liquid for later use; (3) The prepared spinning solution and core solution are respectively fed into a spinneret of a specific size through a gear pump at a certain flow rate and are simultaneously extruded from the spinneret, passed through a certain air gap height under the stretching of a guide wheel, and then enter a coagulation bath to solidify into a hollow fiber membrane; (4) The initially formed hollow fiber membrane is collected on the collection wheel under the traction of the guide wheel and a certain pulling speed; (5) Soaking the collected hollow fiber membrane in pure water for several days, changing the pure water every once in a while, and then washing it several times with non-solvent A and non-solvent B, changing the non-solvent every once in a while; (6) The treated hollow fiber membrane is placed in a vacuum drying oven and dried for a certain period of time.

6. The preparation method according to claim 5, characterized in that: The solvent in step (1) includes but is not limited to N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc) and tetrahydrofuran (THF), and the non-solvent includes but is not limited to water, ethanol, ethyl acetate and acetic acid.

7. The preparation method according to claim 5, characterized in that: The proportions of the spinning solution components in step (1) are as follows: the polymer component content is 20-30wt%, the solvent component content is 40-60wt%, the non-solvent component content is 10-20wt%, and the metal salt component content is 2-5wt%.

8. The preparation method according to claim 5, characterized in that: The solvent content in the core liquid component of step (2) is 10-30wt%; the solvent is selected from one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide and tetrahydrofuran.

9. The preparation method according to claim 5, characterized in that: In step (3), the feed liquid flow rate is 10-15 ml / min, and the core liquid flow rate is 5-10 ml / min; the outer diameter of the spray core is 0.5-1.0 mm, the inner diameter is 0.3-0.8 mm, and the air gap height is 5-15 cm.

10. The preparation method according to claim 5, characterized in that: The stretching speed in step (4) is 15-30 m / min.

11. The preparation method according to claim 5, characterized in that: The soaking time in pure water in step (5) is 3-5 days, and the water is changed every 6-12 hours; the non-solvent A and non-solvent B are cleaned 3-5 times respectively, and changed every 30-60 minutes; the non-solvent A is selected from one of methanol, ethanol and isopropanol; the non-solvent B is selected from one of n-hexane and n-heptane.

12. The preparation method according to claim 5, characterized in that: The specified drying temperature in step (6) is 50-100° C., and the drying time is 12-18 hours.

13. A method for preparing a metal coordinated cross-linked anti-plasticization hollow fiber membrane, characterized in that: The uses of the hollow fiber membrane module include, but are not limited to, natural gas purification, carbon dioxide capture, hydrogen separation and purification, air separation, natural gas helium extraction, gas dehumidification, and olefin and alkane separation.

Citation Information

Patent Citations

  • Structure and preparation method of a gas separation membrane for helium extraction from natural gas with anti-plasticization effect

    CN116272441B

  • High-strength anti-plasticizing gas separation membrane as well as preparation method and application thereof

    CN116407966A

  • A preparation method and application of a hollow fiber membrane with a dense inner surface for gas separation

    CN116943460B

  • Modified chlorinated polyvinyl chloride hollow fiber membrane and preparation process thereof

    CN117101428A

  • Solvent-resistant polymer nanofiltration membrane as well as preparation method and application thereof

    CN111514768A