Preparation method of hydrogel with high mechanical strength and adsorption performance

By preparing composite hydrogels of nanometer graphene oxide, polyvinyl alcohol and other materials, the problems of low efficiency and insufficient mechanical properties of existing technologies in dye wastewater treatment in the textile printing and dyeing industry are solved, achieving both high mechanical strength and adsorption performance. , achieving efficient removal of dyes in dye wastewater.

CN118751202APending Publication Date: 2024-10-11JIANGSU UNIV OF TECH

Patent Information

Application Number
CN202410956786.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively remove industrial dyes such as methylene blue from dye wastewater produced in the textile printing and dyeing industry. Traditional methods are costly and inefficient, and the mechanical properties of hydrogels are insufficient to meet practical application requirements.

Method used

Materials such as nanographene oxide, polyvinyl alcohol, and polyethylene oxide are used to prepare hydrogels with high mechanical strength. Through ultrasonic vibration and freeze-thaw cycle processes, a composite hydrogel with excellent adsorption properties is formed.

Benefits of technology

The prepared hydrogel has a maximum tensile strength of 2MPa and a maximum compressive strength of 13MPa. It also has excellent adsorption properties and can efficiently remove dyes from dye wastewater, solving the problems of high cost and low efficiency of traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118751202A_ABST
    Figure CN118751202A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of hydrogel with high mechanical strength and adsorption performance, and relates to the technical field of biomaterials.The preparation method comprises the following steps that S1, firstly, 0.05 g-0. 25 g of nano graphene oxide is weighed and put into a beaker containing 45 ml of deionized water; putting the beaker into an ultrasonic oscillator, and carrying out ultrasonic treatment for 30 minutes to obtain uniform nano graphene oxide dispersion liquid; s2, weighing 5g of polyvinyl alcohol, pouring into a beaker, putting the beaker into a water bath kettle at 95 DEG C, and stirring for 2 hours; after the polyvinyl alcohol is completely dissolved, adjusting the temperature of the water bath kettle to 70 DEG C, weighing 0.1-0.3 g of polyoxyethylene, pouring the polyoxyethylene into the beaker, and stirring at a low speed until the polyoxyethylene is completely dissolved; then placing the beaker in an ultrasonic oscillator for ultrasonic treatment for 30 min; s3, finally, the prepared emulsion is poured into a polytetrafluoroethylene mold and put into a freeze dryer, samples are taken out every six hours and put into an environment at the temperature of 5 DEG C to be unfrozen for 2 h, the operation is a freeze-thaw cycle, and freeze-thaw is circulated five times.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomaterials, and in particular to a method for preparing a hydrogel with high mechanical strength and adsorption performance. Background Art

[0002] The large amount of organic wastewater generated by the textile printing and dyeing industry will have a serious impact on the ecological environment and human health. The characteristics of dye wastewater are high color and difficult to be naturally biodegraded. It is very harmful to the ecological environment of water bodies and destroys the original ecosystem. Before the wastewater is discharged into the environment and surface water, the adsorption method is generally used to remove the dye in the wastewater.

[0003] The reason why adsorption is widely used in the field of adsorption and removal of dye wastewater is that it is environmentally friendly while being cheaper, more efficient in treating wastewater, and more convenient to operate. At present, common adsorbents mainly use activated carbon with a relatively high surface area or mineral adsorption materials with a layered network structure, while hydrogel is an important new material that is not only widely used in controlled drug release systems, semipermeable membrane products, etc., but can also be used to remove dyes and some heavy metal ions from dye wastewater. In particular, the purification and removal of industrial dye wastewater such as methylene blue (MB) is a very serious environmental problem, because the biological treatment, physical and chemical treatment methods (such as chemical oxidation and filtration) used by traditional industries are difficult to remove methylene blue from it. Summary of the invention

[0004] The object of the present invention is to provide a method for preparing a hydrogel having both high mechanical strength and adsorption performance, so as to solve the problems raised in the above background technology.

[0005] To achieve the above object, the present invention provides the following technical solution: a method for preparing a hydrogel having both high mechanical strength and adsorption performance, comprising the following steps:

[0006] S1. Weigh 0.05g-0.25g of nano-graphene oxide into a beaker containing 45ml of deionized water, and place the beaker in an ultrasonic oscillator for thirty minutes to obtain a uniform nano-graphene oxide dispersion;

[0007] S2. Weigh 5g of polyvinyl alcohol and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the polyvinyl alcohol is completely dissolved, adjust the temperature of the water bath to 70℃, weigh 0.1g-0.3g of polyethylene oxide and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0008] S3. Finally, pour the prepared emulsion into a polytetrafluoroethylene mold and put it into a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle is repeated 5 times.

[0009] Preferably, the content of nano-graphene oxide in the hydrogel is 0.1-0.5wt%, the content of polyvinyl alcohol is 1wt%, and the content of Zr element is 0.2-0.6wt%.

[0010] Compared with the prior art, the present invention has the following beneficial effects:

[0011] The hydrogel has excellent mechanical properties, with a maximum tensile strength of 2MPa, a maximum tensile displacement of 480% of the initial form, and a maximum compressive strength of 13MPa. The hydrogel has both high mechanical strength and excellent adsorption properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 :(a) (c) SEM of PPG hydrogel surface;

[0013] (b) (d) are cross-sectional SEM images of PPG hydrogel, respectively;

[0014] Figure 2 : (a) FTIR spectra of PVA, PP and PPG hydrogels;

[0015] (b) Raman spectra of GO and PPG hydrogels.

[0016] Figure 3 :(a)(b) Tensile stress-strain curves of hydrogels with different components;

[0017] (c) Tensile stress-strain curves of PPG hydrogels with different PEO contents.

[0018] (d) Compressive stress-strain curves of PPG hydrogels with different components;

[0019] Figure 4 :(a) UV-visible spectra of wastewater dye supernatant after adsorption at different temperatures;

[0020] (b) UV-visible spectra of wastewater dye supernatant after adsorption at different pH;

[0021] (c) UV-visible spectra of wastewater dye supernatant after adsorption at different GO contents;

[0022] (d) Local magnification of different GO contents;

[0023] Figure 5 : (a) Pseudo-first-order adsorption kinetics;

[0024] (b) Pseudo-second-order adsorption kinetics;

[0025] (c) Langmuir isotherm adsorption model;

[0026] (d) Freundlich isotherm adsorption model. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] Example 1

[0029] 1. Weigh 0.25 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0030] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.3g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0031] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0032] Example 2

[0033] 1. Weigh 0.2 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0034] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.3g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0035] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0036] Example 3

[0037] 1. Weigh 0.15 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0038] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.2g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0039] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0040] Example 4

[0041] 1. Weigh 0.10 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0042] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.2g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0043] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0044] Example 5.

[0045] 1. Weigh 0.05 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0046] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.1g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0047] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0048] Comparative Example 1

[0049] 1. Weigh 0.25 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0050] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir for 2h. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0051] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0052] Comparative Example 2

[0053] 1. Weigh 0.25 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0054] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.3g of sodium alginate (SA) and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0055] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0056] Comparative Example 3

[0057] 1. Weigh 0.25 g of GO into a beaker containing 45 ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform GO dispersion;

[0058] 2. Next, weigh 5g of PVA and pour it into a beaker. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the PVA is completely dissolved, adjust the temperature of the water bath to 70℃. Then weigh 0.05g of PEO and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min.

[0059] 3. Finally, pour the prepared colloid into a polytetrafluoroethylene mold and place it in a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle should be repeated 5 times.

[0060] The present invention takes Example 1 as the standard and finally successfully prepares a PVA / PEO / GO composite hydrogel with both high mechanical strength and adsorption performance. When PEO is 0.3g and GO reaches 0.25g, the mechanical properties of the hydrogel reach the best maximum tensile strength of 2MPa, and the maximum compressive strength can reach 13MPa; the adsorption effect is also the best.

[0061] In summary, the present invention studies the effects of relevant parameters such as temperature, pH and adsorbent concentration on the adsorption performance through adsorption performance testing, and obtains the optimal temperature, pH and adsorbent concentration for adsorption.

[0062] It is known from common technical knowledge that the present invention can be implemented by other embodiments that do not deviate from its spirit or essential features. Therefore, the above disclosed embodiments are only illustrative in all respects and are not exclusive. All changes within the scope of the present invention or within the scope equivalent to the present invention are included in the present invention.

Claims

1. A method for preparing a hydrogel having both high mechanical strength and adsorption performance, characterized in that: Including the following processes: S1. Weigh 0.05g-0.25g of nano-graphene oxide GO into a beaker containing 45ml of deionized water, and place the beaker in an ultrasonic oscillator for 30 minutes to obtain a uniform nano-graphene oxide dispersion; S2. Weigh 5g of polyvinyl alcohol (PVA) and pour it into the dispersion in S1. Place the beaker in a 95℃ water bath and stir at low speed for 2h. After the polyvinyl alcohol (PVA) is completely dissolved, adjust the temperature of the water bath to 70℃, weigh 0.1g-0.3g of polyethylene oxide (PEO) and pour it into the beaker and stir at low speed until it is completely dissolved. Then place the beaker in an ultrasonic oscillator and ultrasonicate for 30min. S3. Finally, pour the prepared emulsion into a polytetrafluoroethylene mold and put it into a freeze dryer. Take out the sample every six hours and place it in a 5°C environment to thaw for 2 hours. This is a freeze-thaw cycle, and the freeze-thaw cycle is repeated 5 times.

2. The hydrogel prepared by the preparation method according to claim 1, characterized in that: The content of nano graphene oxide in the hydrogel is 0.1-0.5wt%, the content of polyvinyl alcohol is 1wt%, and the content of polyethylene oxide is 0.2-0.6wt%.

Citation Information

Patent Citations

  • Method for preparing polyvinyl alcohol-graphene oxide nano composite hydrogel

    CN106750378A

  • Sericin hydrogel beneficial to multi-tissue repair and preparation method thereof

    CN111228566A

  • Preparation method and application of graphene-modified all-solid-state electrolyte

    CN112259832A

  • Manufacturing method of biocompatible poly(vinyl alcohol)-based hydrogel

    KR1020100118860A

Cited By

  • Complete set of hydrogel particle production equipment and production method

    CN120361796A

  • A complete set of production equipment and production method for hydrogel particles