A catalyst for the low-temperature catalytic oxidation of dimethyl carbonate, its preparation and application
By preparing the LaFe1-xBxO3 catalyst, the problem of low-temperature catalytic oxidation of dimethyl carbonate was solved, achieving efficient catalytic oxidation and degradation at low temperatures, reducing the degradation temperature of dimethyl carbonate and methanol, and exhibiting good selectivity and stability.
Patent Information
- Application Number
- CN202410949470.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-07-16
AI Technical Summary
Existing technologies struggle to efficiently catalyze the oxidation of volatile organic compounds like dimethyl carbonate at low temperatures, and traditional catalysts are costly and have poor performance.
Using LaFe1-xBxO3 (B=Co, Mn, Cu; x=0~0.2) catalyst, perovskite catalyst precursor sol was synthesized by microwave reaction of mixed nitrate, citric acid and polyethylene glycol 2000, and catalyst particles were prepared by adding functional monomers and initiators.
The adsorption and activation of dimethyl carbonate at room temperature were achieved, and the intermediate products were gradually degraded and completely catalytically oxidized to carbon dioxide and water. This significantly reduced the degradation temperature of dimethyl carbonate and methanol, demonstrating high physical stability and selectivity.
Smart Images

Figure CN118751251B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a catalyst for the low-temperature catalytic oxidation of dimethyl carbonate, its preparation and application, and belongs to the fields of environmental protection and thermocatalysis technology. Background Technology
[0002] Volatile organic compounds (VOCs) pose serious threats to ambient air quality and human health. Catalytic oxidation, due to its low temperature, high efficiency, and non-toxic byproducts, has become one of the most promising technologies for VOC removal. Perovskite oxides (ABO3) are inexpensive and widely available. Their tunable elemental composition, flexible structure, and high thermal / chemical stability make them highly efficient and stable catalysts for the catalytic oxidation of VOCs.
[0003] Dimethyl carbonate (DMC) is an excellent methylating agent for VOCs, used in the pharmaceutical and agricultural industries, and widely used as a solvent and carbonylation and methylation agent. Furthermore, DMC is a major solvent in lithium-ion battery electrolytes; the main VOC components in the dismantling process of lithium-ion batteries are esters and benzene, with DMC accounting for the highest proportion, at 65.1% of total VOCs. DMC is also a significant precursor to PM2.5 and ozone, posing a significant threat to the atmospheric environment. PM2.5 can enter the human body through the respiratory tract or skin, seriously harming human health. Summary of the Invention
[0004] The purpose of this invention is to provide a catalyst for the low-temperature catalytic oxidation of dimethyl carbonate, wherein the catalyst is LaFe 1-x B x O3, B = Co, Mn, Cu; x = 0~0.2; This catalyst has a simple preparation process, good low-temperature activity, and excellent VOCs removal performance; In addition, this catalyst has good activity and low price, and can be used on a large scale as an inexpensive support for catalysts.
[0005] Another object of the present invention is to provide a method for preparing the catalyst, wherein a precursor sol is obtained by mixing and reacting different proportions of nitrate compounds, citric acid and polyethylene glycol 2000, followed by stirring, evaporation and microwave synthesis, and then adding functional monomers and initiators to obtain LaFe. 1-x B x O3 (B = Co, Mn, Cu; x = 0, 0.2), specifically includes the following steps:
[0006] (1) Dissolve metal nitrate, citric acid and polyethylene glycol in pure water to obtain a mixture. The molar ratio of metal ions in the metal nitrate is La:Fe:B = 1:0.8:0.2, and the molar ratio of citric acid to total metal cations is 1:1. The amount of polyethylene glycol added to the mixture is 0.02 g / ml.
[0007] (2) Stir the mixture under constant temperature until all reagents are completely dissolved; place it in a microwave reaction device and react at a certain temperature for a period of time to obtain a perovskite catalyst precursor sol.
[0008] (3) Dissolve 0.5 mmol of methacrylic acid as a functional monomer in 10 ml of methanol, sonicate and let stand for later use.
[0009] (4) Dissolve 1 mmol of azobisisobutyronitrile as an initiator in 20 ml of methanol for later use.
[0010] (5) Pour the solutions from steps (3) and (4) into 100 ml of the precursor sol obtained in step (2), sonicate and bathe in water, and finally LaFe 1-x B x O3 is used as a catalyst.
[0011] (6) The catalyst prepared above is pressed into tablets and sieved using a tablet press and a standard sieve to obtain catalyst particles of 40-60 mesh size for later use.
[0012] Preferably, the molecular weight of the polyethylene glycol in this invention is 2000-4000.
[0013] Preferably, the stirring conditions in step (2) of the present invention are constant temperature stirring and heating at 80°C for 8 hours.
[0014] Preferably, the microwave reaction conditions in step (2) of the present invention are 75°C for two hours.
[0015] Preferably, the conditions in step (3) of the present invention are ultrasonic treatment for 30 minutes and standing for 8 hours.
[0016] Preferably, the conditions in step (5) of the present invention are ultrasonic treatment for 30 minutes and water bath at 50°C for 12 hours.
[0017] Another object of the present invention is to provide the application of the catalyst in the low-temperature catalytic oxidation of dimethyl carbonate, wherein the catalytic oxidation process is as follows: using lanthanum ferrite-based perovskite oxide as a catalyst, air is introduced and nitrogen is used as a gas mixture to carry out the catalytic oxidation reaction of dimethyl carbonate.
[0018] The beneficial effects of this invention are as follows:
[0019] (1) The method described in this invention is simple, inexpensive, readily available, high-yield, low-energy-consumption, and environmentally friendly. The lanthanum iron-based perovskite oxide catalyst is used in the catalytic degradation experiment of dimethyl carbonate. The catalyst can adsorb and activate dimethyl carbonate at room temperature and decompose intermediate products. As the temperature increases, the intermediate products and dimethyl carbonate will be gradually degraded until carbon dioxide and water are completely generated, and finally the low-temperature complete catalytic oxidation of dimethyl carbonate is achieved.
[0020] (2) In the catalytic degradation of dimethyl carbonate, lattice oxygen is the most important active substance, and LaFeO3 is an important low-temperature catalyst and a very promising catalyst.
[0021] (3) Compared with the LaFeO3 catalyst, doping other metal elements at the B site can enhance the redox ability of the catalyst, thereby effectively reducing the temperature at which dimethyl carbonate is completely catalytically oxidized.
[0022] (4) The catalyst described in this invention exhibits high physical stability and specific recognition characteristics, and shows good selectivity for methanol, thereby effectively reducing the temperature for complete catalytic oxidation of methanol. Attached Figure Description
[0023] Figure 1 LaFe 1-x B x XRD patterns of O3 (B = Co, Mn, Cu; x = 0, 0.2) catalysts.
[0024] Figure 2 M-LaFe 1-x B x O3 (B = Co, Mn, Cu; x = 0, 0.2) catalyst and blank catalyst activity diagram for catalytic oxidation of 700 ppm dimethyl carbonate.
[0025] Figure 3 M-LaFe 1-x B x Plots showing methanol yields from O3 (B = Co, Mn, Cu; x = 0, 0.2) catalyst and blank catalyst for the catalytic oxidation of 700 ppm dimethyl carbonate.
[0026] Figure 4 M-LaFe 1-x B x Figure 1 shows the CO2 yield of O3 (B = Co, Mn, Cu; x = 0, 0.2) catalyst and blank catalyst for the catalytic oxidation of 700 ppm dimethyl carbonate. Detailed Implementation
[0027] The present invention will be further described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to the content described.
[0028] Example 1
[0029] In Example 1, the molar ratio of La:Fe was 1:1, and the specific operating steps are as follows:
[0030] (1) Weigh 10 mmol (4.33 g) of lanthanum nitrate hexahydrate into a 250 ml beaker, then weigh 10 mmol (4.04 g) of ferric nitrate nonahydrate into the same beaker, then weigh 10 mmol (2.1 g) of citric acid into this beaker, then add 2 g of polyethylene glycol 2000 and add 100 mL of ultrapure water into the beaker as a solvent.
[0031] (2) Seal the mixture with sealing film, and then place the beaker in a constant temperature water bath at 80°C and stir for 8 hours.
[0032] (3) Pour the obtained solution into a 100ml round-bottom flask. The solution should not exceed one-third of the flask volume. Then place the round-bottom flask into a microwave chemical synthesis device, connect a condenser to the circulating water condenser, set the reaction program parameters, and react at 75℃ for two hours. Finally, LaFeO3 sol (denoted as LFO) is obtained.
[0033] (4) Weigh 0.5 mmol (0.043 g) of methacrylic acid (MMA) as a functional monomer, dissolve it in 10 ml of methanol, sonicate for 30 minutes, and then let it stand for 8 hours before use.
[0034] (5) Weigh 1.0 mmol (0.164 g) of azobisisobutyronitrile (AIBN) as an initiator and dissolve it in 20 ml of methanol for later use.
[0035] (6) Pour the solutions from (4) and (5) above into LFO, sonicate for 30 minutes, and then bathe in a water bath at 50°C for 12 hours to finally obtain LaFeO3 (denoted as M-LFO).
[0036] (7) Grind the obtained M-LFO and sieve it through a 40-60 mesh for later use.
[0037] The LaFeO3 prepared in this embodiment was used to test the catalytic oxidation of dimethyl carbonate. This embodiment was completed using equipment built in the laboratory. In the activity test, 0.1g of catalyst was placed in a fixed-bed quartz tube reactor, and the inlet gas flow rate was precisely controlled using a high-precision mass flow meter. N2 was used as the carrier gas, and the gas composition was: dimethyl carbonate 700ppm, O2 2vol%, total flow rate 50ml / min, catalyst dosage 0.1g, and reaction space velocity 30,000mL / (gh). The specific reaction temperature was adjusted by a temperature control device. The detection part consisted of a gas chromatograph and a chromatography workstation. The gas chromatograph included two hydrogen ion flame ionization detectors and a methane conversion furnace, which could detect dimethyl carbonate and CO2. Finally, the standard prepared by the external standard method was converted into specific concentrations.
[0038] Depend on Figure 2 It can be seen that without a catalyst, the complete conversion of dimethyl carbonate is achieved at 325℃, while M-LFO achieves the complete conversion at 200℃, significantly reducing the low-temperature degradation temperature of dimethyl carbonate; Figure 3 It can be seen that without a catalyst, the intermediate product methanol is completely converted at 425℃, while M-LFO achieves complete methanol conversion at 275℃, significantly reducing the methanol degradation temperature; Figure 4 It can be seen that without a catalyst, dimethyl carbonate and methanol are completely catalytically oxidized to CO2 at 500℃ with a CO2 yield of 1. M-LFO completes the deep oxidation of dimethyl carbonate and methanol at 350℃, significantly improving the low-temperature catalytic oxidation effect of dimethyl carbonate and methanol.
[0039] Example 2
[0040] In this embodiment, the molar ratio of La:Fe:Co is 1:0.8:0.2, and the specific operation steps are as follows:
[0041] (1) Weigh 10 mmol (4.33 g) of lanthanum nitrate hexahydrate into a 100 ml beaker, then weigh 8 mmol (3.232 g) of ferric nitrate nonahydrate into the same beaker, then weigh 2 mmol (0.582 g) of cobalt nitrate hexahydrate into the same beaker, and finally weigh 10 mmol (2.1 g) of citric acid as a complexing agent into this beaker, then add 2 g of polyethylene glycol 2000 and add 100 mL of ultrapure water into the beaker as a solvent.
[0042] (2) Seal the mixture with sealing film, and then place the beaker in a constant temperature water bath at 80°C and stir for 8 hours.
[0043] (3) Pour the obtained solution into a 100ml round-bottom flask, ensuring the solution does not exceed one-third of the flask's volume. Then, place the round-bottom flask in a microwave chemical synthesis apparatus, connect a condenser with circulating water for condensation, set the reaction program parameters, and react at 75℃ for two hours; finally, LaFe is obtained. 0.8 Co 0.2 O3 sol (denoted as LFCo).
[0044] (4) Weigh 0.5 mmol (0.043 g) of methacrylic acid (MMA) as a functional monomer, dissolve it in 10 ml of methanol, sonicate for 30 minutes, and then let it stand for 8 hours before use.
[0045] (5) Weigh 1.0 mmol (0.164 g) of azobisisobutyronitrile (AIBN) as an initiator and dissolve it in 20 ml of methanol for later use.
[0046] (6) Pour the solutions from (4) and (5) above into LFCo, sonicate for 30 minutes, and then bathe in a water bath at 50°C for 12 hours to finally obtain LaFe. 0.8 Co 0.2 O3 (denoted as M-LFCo).
[0047] (7) Grind the obtained M-LFCo and sieve it through a 40-60 mesh for later use.
[0048] The LaFe prepared in this embodiment 0.8 Co 0.2 The catalytic oxidation of dimethyl carbonate was tested using O3, and the experimental procedure and conditions were the same as in Example 1.
[0049] Depend on Figure 2 It can be seen that without a catalyst, the complete conversion of dimethyl carbonate is achieved at 325℃, while M-LFCo achieves the complete conversion at 200℃, significantly reducing the low-temperature degradation temperature of dimethyl carbonate; Figure 3 It can be seen that without a catalyst, the intermediate product methanol is completely converted at 425℃, while M-LFCo achieves complete methanol conversion at 200℃, significantly reducing the methanol degradation temperature; Figure 4 It can be seen that without a catalyst, dimethyl carbonate and methanol are completely catalytically oxidized to CO2 at 500℃ with a CO2 yield of 1. M-LFCo, on the other hand, completes the deep oxidation of dimethyl carbonate and methanol at 200℃, significantly improving the low-temperature catalytic oxidation effect of dimethyl carbonate and methanol.
[0050] Example 3
[0051] In this embodiment, the molar ratio of La:Fe:Mn is 1:0.8:0.2, and the specific operation steps are as follows:
[0052] (1) Weigh 10 mmol (4.33 g) of lanthanum nitrate hexahydrate into a 100 ml beaker, then weigh 8 mmol (3.232 g) of ferric nitrate nonahydrate into the same beaker, then weigh 2 mmol (0.502 g) of manganese nitrate tetrahydrate into the same beaker, and finally weigh 10 mmol (2.1 g) of citric acid as a complexing agent into this beaker, then add 2 g of polyethylene glycol 2000 and add 100 mL of ultrapure water into the beaker as a solvent.
[0053] (2) Seal the mixture with sealing film, and then place the beaker in a constant temperature water bath at 80°C and stir for 8 hours.
[0054] (3) Pour the obtained solution into a 100ml round-bottom flask, ensuring the solution does not exceed one-third of the flask's volume. Then, place the round-bottom flask in a microwave chemical synthesis apparatus, connect a condenser with circulating water for condensation, set the reaction program parameters, and react at 75℃ for two hours; finally, LaFe is obtained. 0.8 Mn 0.2 O3 sol (denoted as LFMn).
[0055] (4) Weigh 0.5 mmol (0.043 g) of methacrylic acid (MMA) as a functional monomer, dissolve it in 10 ml of methanol, sonicate for 30 minutes, and then let it stand for 8 hours before use.
[0056] (5) Weigh 1.0 mmol (0.164 g) of azobisisobutyronitrile (AIBN) as an initiator and dissolve it in 20 ml of methanol for later use.
[0057] (6) Pour the solutions from (4) and (5) above into LFMn, sonicate for 30 minutes, and then bathe in a water bath at 50°C for 12 hours to finally obtain LaFe. 0.8 Mn 0.2 O3 (denoted as M-LFMn).
[0058] (7) Grind the obtained M-LFMn and sieve it through a 40-60 mesh for later use.
[0059] The LaFe prepared in this embodiment 0.8 Mn 0.2 The catalytic oxidation of dimethyl carbonate was tested using O3, and the experimental procedure and conditions were the same as in Example 1.
[0060] Depend on Figure 2 It can be seen that without a catalyst, the complete conversion of dimethyl carbonate is achieved at 325℃, while M-LFMn achieves the complete conversion at 200℃, significantly reducing the low-temperature degradation temperature of dimethyl carbonate; Figure 3It can be seen that without a catalyst, the intermediate product methanol is completely converted at 425℃, while M-LFMn completes the methanol conversion at 200℃, significantly reducing the methanol degradation temperature; Figure 4 It can be seen that without a catalyst, dimethyl carbonate and methanol are completely catalytically oxidized to CO2 at 500℃ with a CO2 yield of 1. M-LFMn completes the deep oxidation of dimethyl carbonate and methanol at 200℃, significantly improving the low-temperature catalytic oxidation effect of dimethyl carbonate and methanol.
[0061] Example 4
[0062] In this embodiment, the molar ratio of La:Fe:Cu is 1:0.8:0.2, and the specific operation steps are as follows:
[0063] (1) Weigh 10 mmol (4.33 g) of lanthanum nitrate hexahydrate into a 100 ml beaker, then weigh 8 mmol (3.232 g) of ferric nitrate nonahydrate into the same beaker, then weigh 2 mmol (0.484 g) of copper nitrate trihydrate into the same beaker, and finally weigh 10 mmol (2.1 g) of citric acid as a complexing agent into this beaker, then add 2 g of polyethylene glycol 2000 and add 100 mL of ultrapure water into the beaker as a solvent.
[0064] (2) Seal the mixture with sealing film, and then place the beaker in a constant temperature water bath at 80°C and stir for 8 hours.
[0065] (3) Pour the obtained solution into a 100ml round-bottom flask, ensuring the solution does not exceed one-third of the flask's volume. Then, place the round-bottom flask in a microwave chemical synthesis apparatus, connect a condenser with circulating water for condensation, set the reaction program parameters, and react at 75℃ for two hours; finally, LaFe is obtained. 0.8 Cu 0.2 O3 sol (denoted as LFCu).
[0066] (4) Weigh 0.5 mmol (0.043 g) of methacrylic acid (MMA) as a functional monomer, dissolve it in 10 ml of methanol, sonicate for 30 minutes, and then let it stand for 8 hours before use.
[0067] (5) Weigh 1.0 mmol (0.164 g) of azobisisobutyronitrile (AIBN) as an initiator and dissolve it in 20 ml of methanol for later use.
[0068] (6) Pour the solutions from (4) and (5) above into LFCu, sonicate for 30 minutes, and then bathe in a water bath at 50°C for 12 hours to finally obtain LaFe. 0.8 Cu 0.2 O3 (denoted as LFCu).
[0069] (7) Grind the obtained M-LFCu and sieve it through a 40-60 mesh for later use.
[0070] The LaFe prepared in this embodiment 0.8 Cu 0.2 The catalytic oxidation of dimethyl carbonate was tested using O3, and the experimental procedure and conditions were the same as in Example 1.
[0071] Depend on Figure 2 It can be seen that without a catalyst, the complete conversion of dimethyl carbonate is achieved at 325℃, while M-LFCu achieves the complete conversion at 200℃, significantly reducing the low-temperature degradation temperature of dimethyl carbonate; Figure 3 It can be seen that without a catalyst, the intermediate product methanol is completely converted at 425℃, while M-LFCu achieves complete methanol conversion at 225℃, significantly reducing the methanol degradation temperature; Figure 4 It can be seen that without a catalyst, dimethyl carbonate and methanol are completely catalytically oxidized to CO2 at 500℃ with a CO2 yield of 1. M-LFCu completes the deep oxidation of dimethyl carbonate and methanol at 300℃, significantly improving the low-temperature catalytic oxidation effect of dimethyl carbonate and methanol.
[0072] exist Figure 1 In the middle, the prepared LaFe was compared 1-x B x The XRD pattern of the O3 (B = Co, Mn, Cu; x = 0, 0.2) catalyst clearly shows that the peak positions and shapes of the prepared lanthanum-based perovskite catalyst are basically the same as those in PDF#88-0641; the doped sample has the same pure orthorhombic crystal structure (space group Pnma) as the original LaFeO3 sample, indicating that transition metal doping does not produce impurity peaks. 1-x B x O3 (B = Co, Mn, Cu; x = 0, 0.2) catalysts were successfully prepared, but XRD analysis cannot be directly used as a reference for the performance of the catalyst. Catalyst activity tests are required to determine the specific catalyst activity.
[0073] Comparative Example 1
[0074] In Comparative Example 1, the molar ratio of La:Fe:Mn was 1:0.8:0.2, the same as in Example 3. The specific operating steps are as follows:
[0075] (1) Weigh 10 mmol (4.33 g) of lanthanum nitrate hexahydrate into a 100 ml beaker, then weigh 8 mmol (3.232 g) of ferric nitrate nonahydrate into the same beaker, then weigh 2 mmol (0.502 g) of manganese nitrate tetrahydrate into the same beaker, and finally weigh 10 mmol (2.1 g) of citric acid as a complexing agent into this beaker, and add 100 mL of ultrapure water into the beaker as a solvent.
[0076] (2) Place the mixture on a magnetic stirrer and stir at room temperature for 1 hour until the drug is completely dissolved. Then transfer the beaker to a constant temperature water bath and stir and heat at 80°C to evaporate the solvent until a wet gel is formed. Place the obtained wet gel in a forced-air drying oven and dry at 150°C for 10 hours to form a porous and fluffy dry gel.
[0077] (3) Grind the obtained dry gel thoroughly into powder using a mortar and pestle, place the powder in a crucible, place the crucible in a muffle furnace and heat it to 650°C at 2°C / min and calcine it at a constant temperature for 3 hours.
[0078] (4) The obtained LaFe 0.8 Co 0.2 O3 is ground and sieved through a 40-60 mesh for later use.
[0079] The LaFe prepared in this embodiment 0.8 Cu 0.2 The catalytic oxidation of dimethyl carbonate was tested using O3, and the experimental procedure and conditions were the same as in Example 1.
[0080] By comparing with Example 3, it can be seen that the low-temperature degradation effect of dimethyl carbonate and methanol is not as good as that of Example 3, indicating that the method in Example 3 successfully achieved good selectivity for methanol and reduced the temperature for complete catalytic oxidation of dimethyl carbonate.
[0081] In summary, the lanthanum ferrite-based perovskite oxide prepared in this invention can achieve low-temperature complete catalytic oxidation of dimethyl carbonate. Furthermore, the preparation method is simple, inexpensive, readily available, has high yield, low energy consumption, and is environmentally friendly. Doping the catalyst at the B-site with metal elements can significantly optimize the low-temperature catalytic degradation effect of dimethyl carbonate, exhibiting good selectivity for methanol and effectively reducing the temperature for complete catalytic oxidation of methanol. In Example 3, M-LFMn showed the best low-temperature complete catalytic oxidation effect on dimethyl carbonate.
Claims
1. A method for preparing a catalyst for the low-temperature catalytic oxidation of dimethyl carbonate, characterized in that, Specifically, the following steps are included: (1) A mixture was obtained by dissolving metal nitrate, citric acid and polyethylene glycol in pure water. The molar ratio of metal ions in the metal nitrate was La:Fe:B = 1:0.8:0.2, and the molar ratio of citric acid to total metal cations was 1:
1. The amount of polyethylene glycol added to the mixture was 0.02 g / ml. (2) Stir the mixture under constant temperature until all reagents are completely dissolved; place it in a microwave reaction device and react at a certain temperature for a period of time to obtain a perovskite catalyst precursor sol; (3) Dissolve 0.5 mmol of methacrylic acid as a functional monomer in 10 ml of methanol, sonicate and let stand for later use; (4) Dissolve 1 mmol of azobisisobutyronitrile as an initiator in 20 ml of methanol for later use; (5) Pour the solutions from steps (3) and (4) above into 100 ml of the precursor sol obtained in step (2), sonicate and bathe in water to finally obtain the catalyst; the catalyst is LaFe 1-x B x O3, where B = Co, Mn, Cu; x = 0.2; (6) The catalyst prepared above is pressed into tablets and sieved using a tablet press and a standard sieve to obtain catalyst particles of 40-60 mesh size for later use.
2. The method according to claim 1, characterized in that: The molecular weight of polyethylene glycol is 2000-4000.
3. The method according to claim 1, characterized in that: In step (2), the stirring conditions are constant temperature stirring and heating at 80℃ for 8 hours.
4. The method according to claim 1, characterized in that: The microwave reaction conditions in step (2) are 75°C for two hours.
5. The method according to claim 1, characterized in that: The conditions in step (3) are ultrasonic treatment for 30 minutes and standing for 8 hours.
6. The method according to claim 1, characterized in that: The conditions in step (5) are ultrasonic treatment for 30 minutes and water bath at 50°C for 12 hours.
7. The application of the catalyst prepared by the method according to any one of claims 1 to 6 in the low-temperature catalytic oxidation of dimethyl carbonate.