Method and system for removing oxides on surface of nuclear power material
Through chemical reagent pretreatment and laser single pulse testing, the parameters of the spot-free overlapping process were determined, and combined with the use of low-power lasers, the problem of low laser decontamination efficiency in the existing technology was solved, and the effect of efficient removal of surface oxides of nuclear power materials was achieved. .
Patent Information
- Application Number
- CN202410740504.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-08
- Publication Date
- 2024-10-11
AI Technical Summary
Existing laser decontamination technology has low efficiency in removing oxides from the surface of nuclear power materials. This is mainly due to the reduction in scanning speed and line spacing caused by the spot overlap rate, which affects the removal efficiency.
After pretreatment with chemical reagents, the scanning process parameters of no spot overlap are determined through laser single pulse testing, and the process plan of no spot overlap is designed to achieve full scanning removal. Combined with the combined use of low-power lasers and chemical reagents, the removal efficiency is improved. And reduce laser energy consumption.
It significantly improves the decontamination efficiency, reduces laser energy consumption, enables low-power lasers to achieve the removal efficiency of high-power lasers, and optimizes the decontamination effect.
Smart Images

Figure CN118751613A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of removing oxides from the surface of nuclear power materials, and in particular relates to a method and a system for removing oxides from the surface of nuclear power materials. Background Art
[0002] Nuclear facility maintenance, decommissioning and emergency response all require decontamination to prevent radioactive substances from polluting the environment and harming human health, reduce the waste dose exposed to the environment, and achieve the purpose of recycling equipment and materials. Most radioactive substances exist in the oxide layer generated on the surface of nuclear facilities due to long-term water chemical conditions. Therefore, removing the surface oxide layer can remove most radioactive substances.
[0003] As a new decontamination method, laser decontamination has the advantages of good decontamination effect, little damage to the substrate, less secondary waste, and remote operation and automation. It is an effective method to meet the deradioactivity requirements of nuclear facilities.
[0004] At present, most of the laser decontamination research is a single laser treatment, or a single chemical decontamination method, with average decontamination efficiency, which is still far from the efficiency required for actual production applications. Regarding the current laser decontamination research, for actual production applications, the prior art has an invention patent "Precise and non-destructive laser decontamination method for contaminated metal parts on the surface of nuclear facilities" (202110364548.4) that proposes a nanosecond + picosecond laser decontamination process, and its decontamination efficiency is only 1.728m 2 / h, and according to previous experimental exploration, one of the reasons for limiting efficiency is the laser removal process with spot overlap rate, because this will reduce the laser scanning speed and line spacing, thereby greatly reducing the laser removal efficiency. Therefore, further proposing an efficient decontamination method is an issue that needs to be improved in practical applications. Summary of the invention
[0005] The purpose of the present invention is to provide a system and method for removing oxides from the surface of nuclear power materials, so as to further improve the decontamination effect and decontamination efficiency.
[0006] To solve the above problems, one aspect of the present invention provides a method for removing oxides on the surface of nuclear power materials, comprising the following steps:
[0007] Spray chemical reagents onto the surface of the material to be decontaminated;
[0008] Set laser parameters and perform a laser single pulse test on the surface of the material to be decontaminated;
[0009] Record the action range of a single laser pulse and calculate the scanning process parameters without spot overlap based on the action range;
[0010] Set the scanning process parameters and use the laser to perform full scanning and removal of the material to be decontaminated.
[0011] The method of removing oxides on the surface of nuclear power materials of the present invention has the beneficial effect that before the material to be decontaminated is subjected to full coverage scanning by laser action, chemical reagents are first sprayed on its surface and left to stand for a while. The chemical reagents can make the oxides loose or react with them so that part of the oxides are separated from the material to be decontaminated, thereby realizing the pretreatment of chemically removing oxides. By utilizing the characteristic that the action area of a single laser pulse on the oxide is larger than its own spot diameter, the action range of a single laser pulse on the material to be decontaminated is explored through a single pulse test, and the scanning process parameters required when the action range overlaps are calculated. In this way, a process scheme without spot overlap is designed, and then the laser is used to perform full scanning and removal of oxides on the surface of the material to be decontaminated, thereby realizing comprehensive laser scanning of the material. The process scheme without overlap can reduce the number of laser actions, and can enable a low-power laser to achieve the removal efficiency of a high-power laser. The combination of chemical reagents and lasers can achieve efficient removal, further improving efficiency, while significantly reducing the consumption of laser energy, and being more energy-efficient.
[0012] In some embodiments, the step of recording the action range of a single laser pulse and calculating scanning process parameters without spot overlap according to the action range includes:
[0013] A CCD camera is used to measure in real time the range of action of a single laser pulse on the surface of the material to be decontaminated;
[0014] The spot action diameter is recorded according to the action range, and the corresponding laser scanning speed and line spacing that can make the spot action areas overlap with each other are calculated to determine the scanning process parameters without spot overlap.
[0015] It can be calculated by the following formula:
[0016]
[0017] Among them, U P is the overlap rate in the laser scanning direction, U L is the overlap rate in the vertical scanning direction, v is the laser scanning speed, D is the spot action diameter, f is the laser frequency, and L is the line spacing of the laser scanning. Substitute the determined spot action diameter and laser frequency to determine the scanning speed and line spacing of the spot-free overlap process.
[0018] Therefore, in the laser single pulse test mode, the laser pulse width and frequency are set, and the laser single pulse is applied to the material to be decontaminated by adjusting different laser powers. The action range of the laser single pulse is observed under the CCD camera, the spot action diameter is recorded, and the corresponding laser scanning speed and line spacing that can make the spot action areas overlap with each other are calculated to determine the laser removal process without spot overlap.
[0019] In some embodiments, the step of setting scanning process parameters and using laser to perform full scanning removal of the material to be decontaminated includes:
[0020] Enter the laser scanning speed and line spacing corresponding to the scanning process parameters without spot overlap, and set the laser power, laser repetition frequency and pulse width;
[0021] Determine the shape, size and filling method of the area to be scanned by the laser according to the size of the material to be decontaminated;
[0022] Use the laser to scan the entire surface of the material to be decontaminated.
[0023] Thus, the full scanning mode is entered, the laser removal process begins, the laser emits light, and scans according to the predetermined working path to achieve full coverage of the laser effect on the material to be decontaminated.
[0024] In some embodiments, the method for removing oxides on the surface of nuclear power materials further comprises:
[0025] Spray protective gas onto the surface of the material to be decontaminated.
[0026] Therefore, it is used to blow away the oxide particles stripped off by the laser to prevent them from adhering to the surface of nuclear power materials. At the same time, it reduces the oxygen content around the laser-cleaned nuclear power materials, inhibits the secondary oxidation of nuclear power materials, and reduces matrix damage.
[0027] In some embodiments, the method for removing oxides on the surface of nuclear power materials further comprises:
[0028] The removed substances are sucked off the surface of the material to be decontaminated.
[0029] Therefore, it is used to absorb the removed objects during the laser removal process to prevent them from causing harm to personnel and the environment.
[0030] In some embodiments, the method for removing oxides on the surface of nuclear power materials further comprises:
[0031] The surface oxide removal effect of the material to be decontaminated is detected. If the removal effect meets the standard, the removal operation is terminated. If it does not meet the standard, jump to the step of setting the scanning process parameters and use the laser to perform a full scan and removal of the material to be decontaminated.
[0032] Therefore, by testing the cleaning and removal effects, adjusting the laser parameters and scanning parameters according to the cleaning effects, the process is continuously optimized to further improve the decontamination effect.
[0033] Another aspect of the present invention provides a system for removing oxides from the surface of nuclear power materials, comprising:
[0034] A laser light source module, used for generating laser;
[0035] An optical path module, used for adjusting the laser optical path generated by the laser light source module and irradiating the laser to the surface of the material to be decontaminated;
[0036] Information processing module, used to set laser parameters and scanning process parameters;
[0037] A chemical reagent spraying module is used to spray chemical reagents on the surface of the material to be decontaminated;
[0038] A testing module, connected to the information processing module, for testing the range of action of a single laser pulse and transmitting the test result to the information processing module;
[0039] The mechanical motion module is connected to the optical path module and the information processing module, and is used to control the movement of the optical path module according to the information transmitted by the information processing module, so as to perform full scanning and removal of the contamination-removing material.
[0040] Therefore, before the laser action is fully covered and scanned on the material to be decontaminated, the chemical reagent spraying module first sprays the chemical reagent on its surface and leaves it for a while. The chemical reagent can make the oxide loose or react with it so that part of the oxide is separated from the material to be decontaminated, thus realizing the pretreatment of chemical removal of oxide; the test module tests the action range of the laser single pulse and transmits the test result to the information processing module, and then the information processing module, the mechanical motion module, the laser light source module and the optical path module jointly complete the full scanning and removal of the oxide on the surface of the material to be decontaminated, thus realizing the comprehensive laser scanning of the material. The non-overlapping process can reduce the number of laser actions, enable low-power lasers to achieve the removal efficiency of high-power lasers, and the combination of chemical reagents and lasers can achieve efficient removal, further improving the efficiency, while significantly reducing the consumption of laser energy, and being more energy-efficient.
[0041] In some embodiments, the system for removing oxides from the surface of nuclear power materials further includes a protective gas module for spraying protective gas onto the material to be decontaminated, thereby blowing away the oxide particles stripped by the laser to prevent them from adhering to the surface of the nuclear power material, while reducing the oxygen content around the laser-cleaned nuclear power material, inhibiting secondary oxidation of the nuclear power material, and reducing matrix damage.
[0042] In some embodiments, the system for removing oxides from the surface of nuclear power materials further includes a dust suction module for sucking out the removed matter stripped off the surface of the material to be decontaminated, thereby absorbing the removed matter stripped off during the laser removal process to prevent it from causing harm to personnel and the environment.
[0043] In some embodiments, the system for removing oxides on the surface of nuclear power materials further includes a detection module, which is used to detect the removal effect of the surface oxides of the material to be decontaminated and transmit the removal effect information to the information processing module, thereby continuously optimizing the removal process and further improving the decontamination effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 A schematic diagram of a method for removing oxides on the surface of nuclear power materials according to an embodiment of the present invention;
[0045] Figure 2 This is the initial surface morphology of the oxide of 304L stainless steel sample;
[0046] Figure 3 The surface morphology of the oxide removed from the 304L stainless steel nuclear power environment simulation sample in Experiment 1 with a laser power of 120W;
[0047] Figure 4 This is the initial surface morphology of the oxide of 17-4PH stainless steel sample;
[0048] Figure 5 The surface morphology of the oxide removed from the sample simulating the nuclear power environment of 17-4PH by laser power of 120W in Experiment 2;
[0049] Figure 6 The surface morphology of the oxide removed from the 304L stainless steel nuclear power environment simulation sample by hydrochloric acid reagent in Experiment 3;
[0050] Figure 7 This is the surface morphology of the oxide removed from the 304L stainless steel nuclear power environment simulation sample after being sprayed with hydrochloric acid reagent using a laser power of 80W in Experiment 3. DETAILED DESCRIPTION
[0051] The present invention will be further described in detail below in conjunction with the accompanying drawings.
[0052] Figure 1 The method for removing oxides from the surface of nuclear power materials according to one embodiment of the present invention is schematically shown. Figure 1 As shown, the method includes:
[0053] S1. Spray chemical reagents onto the surface of the material to be decontaminated;
[0054] S2. Setting laser parameters and performing a laser single pulse test on the surface of the material to be decontaminated;
[0055] S3, recording the action range of the laser single pulse, and calculating the scanning process parameters without spot overlap according to the action range;
[0056] S4. Set scanning process parameters and use laser to perform full scanning and removal of the material to be decontaminated.
[0057] In order to verify the removal effect and efficiency, non-radioactive simulated samples were prepared as the materials to be decontaminated. By simulating the water chemical conditions of the first-loop of nuclear power, non-radioactive samples were prepared using two materials, 304L stainless steel and 17-4PH stainless steel, which are representative materials of nuclear power. The preparation process was carried out in a high-pressure reactor, and the continuous corrosion time was 960 hours.
[0058] Before laser treatment, chemical reagents are sprayed on the surface of the sample. The sprayed chemical reagents can make the oxide loose or react with it to make part of the oxide detach from the oxidized sample, thus realizing the pretreatment of chemical oxide removal. Taking advantage of the characteristic that the laser single pulse has a larger spot diameter in the oxide action area, the single pulse test is used to explore the action range of the laser single pulse on the sample, so as to calculate the scanning process parameters required when the action range overlaps, and design a process plan without spot overlap. Then, the laser is used to perform a full scan to remove the oxide on the surface of the sample, thus realizing a comprehensive laser scan of the material. The non-overlapping process plan can reduce the number of laser actions, and enable low-power lasers to achieve the removal efficiency of high-power lasers. The combination of chemical reagents and lasers can achieve efficient removal, further improving efficiency, while significantly reducing laser energy consumption and saving energy.
[0059] Specifically, the above step S3 includes the following steps:
[0060] A CCD camera is used to measure in real time the range of action of a single laser pulse on the surface of the material to be decontaminated;
[0061] The spot action diameter is recorded according to the action range, and the corresponding laser scanning speed and line spacing that can make the spot action areas overlap with each other are calculated to determine the scanning process parameters without spot overlap.
[0062] Specifically, the spot action diameter is recorded according to the action range, and the overlap rate formula along the laser scanning direction and the vertical scanning direction is used to calculate the corresponding laser scanning speed and line spacing that can make the spot action area overlap with each other. The formula is as follows:
[0063]
[0064] Among them, U P is the overlap rate in the laser scanning direction, U L is the overlap rate in the vertical scanning direction, v is the laser scanning speed, D is the spot action diameter, f is the laser frequency, and L is the line spacing of the laser scanning. Substitute the determined spot action diameter and laser frequency to determine the scanning speed and line spacing of the spot-free overlap process.
[0065] Therefore, in the laser single pulse test mode, the laser pulse width and frequency are set, and the sample is subjected to a single laser pulse by adjusting different laser powers. The action range of the laser single pulse is observed under the CCD camera, the spot action diameter is recorded, and the corresponding laser scanning speed and line spacing that can allow the spot action areas to overlap with each other are calculated to determine the laser removal process without spot overlap.
[0066] Furthermore, the above step S4 includes the following steps:
[0067] Enter the laser scanning speed and line spacing corresponding to the scanning process parameters without spot overlap, and set the laser power, laser repetition frequency and pulse width;
[0068] Determine the shape, size and filling method of the area to be scanned by the laser according to the size of the material to be decontaminated;
[0069] Use the laser to scan the entire surface of the material to be decontaminated.
[0070] Thus, the full scanning mode is entered, the laser removal process begins, the laser emits light, and scans according to the predetermined working path to achieve full coverage of the laser effect on the simulated sample.
[0071] Preferably, the method for removing oxides on the surface of nuclear power materials also includes:
[0072] Spraying protective gas onto the surface of the material to be decontaminated;
[0073] Absorb the removed materials stripped from the surface of the material to be decontaminated. Therefore, it is used to blow away the oxide particles stripped by the laser to prevent them from adhering to the surface of the nuclear power material, while reducing the oxygen content around the laser-cleaned nuclear power material, inhibiting the secondary oxidation of the nuclear power material, and reducing the damage to the matrix; and it is used to absorb the removed materials stripped during the laser removal process to prevent them from causing harm to personnel and the environment.
[0074] More preferably, the method for removing oxides on the surface of nuclear power materials further comprises:
[0075] Detect the surface oxide removal effect of the material to be decontaminated. If the removal effect meets the standard, the removal operation is terminated. If it does not meet the standard, jump to the step to set the scanning process parameters and use the laser to perform a full scan removal of the material to be decontaminated. Therefore, by detecting the cleaning removal effect, adjusting the laser parameters and scanning parameters according to the cleaning effect, continuously optimizing the process, and further improving the decontamination effect.
[0076] When doing a specific experiment, the following practical steps are included:
[0077] Turn on the system power, start the machine, and open the control software on the computer;
[0078] Open the gas cylinder, adjust the gas pressure, and the protective gas system is ready;
[0079] Draw a simple graph in the control software, turn on the collimated light, and adjust the mechanical motion module so that the size of the collimated light graph is consistent with the software setting;
[0080] Open the door of the studio, place the sample on the workbench, prepare hydrochloric acid reagent for the oxide of stainless steel material, spray the chemical reagent, and let it stand for a while;
[0081] The system was set to single pulse test mode, with a fixed laser repetition frequency of 40kHz and a laser pulse width of 500ns. The laser power was used as a variable to perform a single laser pulse on the sample surface. The laser single pulse action diameter was measured by a CCD camera, and the laser removal process with no spot overlap in the action area was calculated and designed.
[0082] Use computer software to draw a 30mm×20mm rectangle, select unidirectional filling, use laser power as a variable, laser scanning speed 15000mm / s, laser scanning line spacing 0.2mm, and the laser removal efficiency under this process is set to a target value of 10m 2 / h, turn on the collimated light to verify the laser scanning range;
[0083] Rotate the air pipe valve to adjust the appropriate airflow;
[0084] Close the studio door, start the laser removal process under the control of the operating software, and the laser emits light to perform a full scan according to the predetermined working path;
[0085] After the laser removal process is completed, turn off the protective gas. After the experiment is completed, close the software, shut down the computer, and turn off the system power.
[0086] The present invention also provides a system for removing oxides on the surface of nuclear power materials, comprising:
[0087] A laser light source module, used for generating laser;
[0088] An optical path module, used for adjusting the laser optical path generated by the laser light source module and irradiating the laser to the surface of the material to be decontaminated;
[0089] Information processing module, used to set laser parameters and scanning process parameters;
[0090] A chemical reagent spraying module is used to spray chemical reagents on the surface of the material to be decontaminated;
[0091] A testing module, connected to the information processing module, for testing the range of action of a single laser pulse and transmitting the test result to the information processing module;
[0092] The mechanical motion module is connected to the optical path module and the information processing module, and is used to control the movement of the optical path module according to the information transmitted by the information processing module, so as to perform full scanning and removal of the contamination-removing material.
[0093] Therefore, before the laser action is fully covered and scanned on the material to be decontaminated, the chemical reagent spraying module first sprays the chemical reagent on its surface and leaves it for a while. The chemical reagent can make the oxide loose or react with it so that part of the oxide is separated from the material to be decontaminated, thus realizing the pretreatment of chemical removal of oxide; the test module tests the action range of the laser single pulse and transmits the test result to the information processing module, and then the information processing module, the mechanical motion module, the laser light source module and the optical path module jointly complete the full scanning and removal of the oxide on the surface of the material to be decontaminated, thus realizing the comprehensive laser scanning of the material. The non-overlapping process can reduce the number of laser actions, enable low-power lasers to achieve the removal efficiency of high-power lasers, and the combination of chemical reagents and lasers can achieve efficient removal, further improving the efficiency, while significantly reducing the consumption of laser energy, and being more energy-efficient.
[0094] Preferably, the system for removing oxides from the surface of nuclear power materials also includes a protective gas module for spraying protective gas onto the material to be decontaminated, thereby blowing away the oxide particles stripped by the laser to prevent them from adhering to the surface of the nuclear power material, while reducing the oxygen content around the laser-cleaned nuclear power material, inhibiting the secondary oxidation of the nuclear power material, and reducing the damage to the matrix.
[0095] Preferably, the system for removing oxides from the surface of nuclear power materials also includes a dust suction module for sucking out the removed matter stripped off the surface of the material to be decontaminated, thereby absorbing the removed matter stripped off during the laser removal process to prevent it from causing harm to personnel and the environment.
[0096] Further preferably, the system for removing oxides on the surface of nuclear power materials also includes a detection module, which is used to detect the removal effect of the surface oxides of the material to be decontaminated, and transmit the removal effect information to the information processing module, thereby continuously optimizing the removal process and further improving the decontamination effect.
[0097] The following specific experiments are conducted to verify the removal effect of the combined use of chemical reagents and lasers:
[0098] Experiment 1
[0099] The laser power is 120W to remove the oxide of 304L stainless steel nuclear power environment simulation sample. The operation steps are as follows:
[0100] Turn on the power, start the machine, turn on the optical path module where the laser and the scanning galvanometer are located, set the lens focal length of the scanning galvanometer to 160mm, and the circular laser spot diameter to 50μm. Turn on the computer and display, and open the control software;
[0101] Open the gas cylinder, adjust the gas pressure, and the protective gas system is ready;
[0102] Draw a simple graph in the control software, turn on the collimated light, and adjust the mechanical motion module so that the size of the collimated light graph is consistent with the software setting;
[0103] Open the door of the studio, place the sample on the workbench, adjust the system to the single pulse test mode, fix the laser repetition frequency at 40kHz and the laser pulse width at 500ns, use the laser power as a variable, perform a single laser pulse on the sample surface, measure the laser single pulse action diameter with a CCD camera, calculate and design a laser removal process with no spot overlap in the action area coverage;
[0104] Use computer software to draw a 30mm×20mm rectangle, select one-way filling, set the laser power to 120W, the laser scanning speed to 15000mm / s, and the laser scanning line spacing to 0.2mm. The laser removal efficiency under this process is greater than 10m 2 / h. Turn on the collimated light to verify the laser scanning range;
[0105] Rotate the air pipe valve to adjust the appropriate airflow;
[0106] Close the studio door, operate the software to start the laser removal process, the laser emits light, scans along the predetermined path, and completes the laser removal process;
[0107] After the laser removal process is completed, turn off the protective gas.
[0108] like Figure 2 The initial surface morphology of the oxide of the 304L stainless steel nuclear power environment simulation sample is as follows: Figure 3 The figure shows the surface morphology of the oxide removed from a 304L stainless steel nuclear power environment simulation sample with a laser power of 120W. Figure 3 and Figure 2 By comparison, it was found that the laser removal process without spot overlap completely removed the oxide on the surface of the sample, and there was a remelting phenomenon on the surface of the sample. This laser power was sufficient to remove the oxide from 304L stainless steel.
[0109] Experiment 2
[0110] The laser power is 120W to remove the oxide of 17-4PH stainless steel nuclear power environment simulation sample. The operation steps are as follows:
[0111] Turn on the power, start the machine, turn on the optical path module where the laser and the scanning galvanometer are located, set the lens focal length of the scanning galvanometer to 160mm, and the circular laser spot diameter to 50μm. Turn on the computer and display, and open the control software;
[0112] Open the gas cylinder, adjust the gas pressure, and the protective gas system is ready;
[0113] Draw a simple graph in the control software, turn on the collimated light, and adjust the mechanical motion module so that the size of the collimated light graph is consistent with the software setting;
[0114] Open the door of the studio, place the sample on the workbench, adjust the system to the single pulse test mode, fix the laser repetition frequency at 40kHz and the laser pulse width at 500ns, use the laser power as a variable, perform a single laser pulse on the sample surface, measure the laser single pulse action diameter with a CCD camera, calculate and design a laser removal process with no spot overlap in the action area coverage;
[0115] Use computer software to draw a 30mm×20mm rectangle, select one-way filling, set the laser power to 120W, the laser scanning speed to 15000mm / s, and the laser scanning line spacing to 0.2mm. The laser removal efficiency under this process is greater than 10m 2 / h. Turn on the collimated light to verify the laser scanning range;
[0116] Rotate the air pipe valve to adjust the appropriate airflow;
[0117] Close the studio door, operate the software to start the laser removal process, the laser emits light, scans along the predetermined path, and completes the laser removal process;
[0118] After the laser removal process is completed, turn off the protective gas.
[0119] Figure 4 The initial surface morphology of the oxide of the 17-4PH stainless steel nuclear power environment simulation sample is as follows: Figure 5 The figure shows the surface morphology of the oxide removed from a 17-4PH stainless steel nuclear power environment simulation sample with a laser power of 140W. Figure 5 and Figure 4 By comparison, it was found that the laser removal process without spot overlap completely removed the oxides on the surface of the sample, and this laser power was sufficient to remove the oxides of 17-4PH stainless steel.
[0120] Experiment 3
[0121] Chemical reagents and laser composite removal of oxides from 304L stainless steel nuclear power environment simulation samples, the operation steps are as follows:
[0122] Turn on the system power, start the machine, and open the control software on the computer;
[0123] Open the gas cylinder, adjust the gas pressure, and the protective gas system is ready;
[0124] Draw a simple graph in the control software, turn on the collimated light, and adjust the mechanical motion module so that the size of the collimated light graph is consistent with the software setting;
[0125] Open the door of the studio, place the sample on the workbench, prepare hydrochloric acid reagent for the oxide of stainless steel material, spray the chemical reagent, let it stand for a while, and the surface morphology of the sample is as follows: Figure 6 As shown, compared Figure 2 It was found that hydrochloric acid reagent can strip oxides to a certain extent, and some oxides fell off on the surface of the sample;
[0126] The system was set to single pulse test mode, with a fixed laser repetition frequency of 40kHz and a laser pulse width of 500ns. The laser power was used as a variable to perform a single laser pulse on the sample surface. The laser single pulse action diameter was measured by a CCD camera, and the laser removal process with no spot overlap in the action area was calculated and designed.
[0127] Use computer software to draw a 30mm×20mm rectangle, select one-way filling, set the laser power to 80W, the laser scanning speed to 15000mm / s, and the laser scanning line spacing to 0.2mm. The laser removal efficiency under this process is greater than 10m 2 / h, turn on the collimated light to verify the laser scanning range;
[0128] Rotate the air pipe valve to adjust the appropriate airflow;
[0129] Close the studio door, start the laser removal process under the control of the operating software, and the laser emits light and scans according to the predetermined working path;
[0130] After the laser removal process is completed, turn off the protective gas.
[0131] The surface morphology of the sample after laser removal is as follows Figure 7 As shown, compared Figure 2 and Figure 6 It was found that the oxide was completely removed after the laser power was applied, and only 80W of laser power was required to achieve this. Figure 5 For the removal of oxides with a laser power of 120W, the chemical + laser composite removal method can further reduce the power of the laser used and achieve better removal effects.
[0132] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed herein, and all embodiments falling within the scope of the claims of this application belong to the scope of protection of the present invention.
Claims
1. A method for removing oxides from the surface of nuclear power materials, It is characterized in that The steps include: Spray chemical reagents onto the surface of the material to be decontaminated; Set laser parameters and perform a laser single pulse test on the surface of the material to be decontaminated; Record the action range of a single laser pulse and calculate the scanning process parameters without spot overlap based on the action range; Set the scanning process parameters and use the laser to perform full scanning and removal of the material to be decontaminated.
2. The method for removing oxides from the surface of nuclear power materials according to claim 1, It is characterized in that Record the action range of the laser single pulse and calculate the scanning process parameters without spot overlap based on the action range, including: A CCD camera is used to measure in real time the range of action of a single laser pulse on the surface of the material to be decontaminated; The spot action diameter is recorded according to the action range, and the corresponding laser scanning speed and line spacing that can make the spot action areas overlap with each other are calculated to determine the scanning process parameters without spot overlap.
3. The method for removing oxides from the surface of nuclear power materials according to claim 2, It is characterized in that Set scanning process parameters and use laser to perform full scanning removal of the material to be decontaminated, including: Enter the laser scanning speed and line spacing corresponding to the scanning process parameters without spot overlap, and set the laser power, laser repetition frequency and pulse width; Determine the shape, size and filling method of the area to be scanned by the laser according to the size of the material to be decontaminated; Use the laser to scan the entire surface of the material to be decontaminated.
4. The method for removing oxides from the surface of nuclear power materials according to claim 1, It is characterized in that The method further comprises: Spray protective gas onto the surface of the material to be decontaminated.
5. The method for removing oxides from the surface of nuclear power materials according to claim 4, It is characterized in that The method further comprises: The removed substances are sucked off the surface of the material to be decontaminated.
6. The method for removing oxides from the surface of nuclear power materials according to claim 1, It is characterized in that The method further comprises: The surface oxide removal effect of the material to be decontaminated is detected. If the removal effect meets the standard, the removal operation is terminated. If it does not meet the standard, jump to the step of setting the scanning process parameters and use the laser to perform a full scan and removal of the material to be decontaminated.
7. A system for removing oxides from the surface of nuclear power materials, It is characterized in that include: A laser light source module, used for generating laser; An optical path module, used for adjusting the laser optical path generated by the laser light source module and irradiating the laser to the surface of the material to be decontaminated; Information processing module, used to set laser parameters and scanning process parameters; A chemical reagent spraying module is used to spray chemical reagents on the surface of the material to be decontaminated; A testing module, connected to the information processing module, for testing the range of action of a single laser pulse and transmitting the test result to the information processing module; The mechanical motion module is connected to the optical path module and the information processing module, and is used to control the movement of the optical path module according to the information transmitted by the information processing module, so as to perform full scanning and removal of the material to be decontaminated.
8. The system for removing oxides from the surface of nuclear power materials according to claim 7, It is characterized in that Also included is a protective gas module for blowing protective gas toward the material to be decontaminated.
9. The system for removing oxides from the surface of nuclear power materials according to claim 7, It is characterized in that It also includes a dust suction module for sucking away the removed matter peeled off from the surface of the material to be decontaminated.
10. A system for removing oxides from the surface of nuclear power materials according to any one of claims 7 to 9, It is characterized in that It also includes a detection module, which is used to detect the surface oxide removal effect of the material to be decontaminated and transmit the removal effect information to the information processing module.
Citation Information
Patent Citations
Accurate nondestructive laser decontamination method for contaminated metal parts on surface of nuclear facilities
CN112845392A
Pre-welding laser cleaning method and device capable of efficiently removing aluminum alloy oxidation film
CN108031687A
Nanosecond laser substrate pretreatment method for improving bonding property of boron-doped diamond electrode film substrate
CN108315711A
Machining method for laser oblique impact strengthening of complex parts
CN109355490A
Method for cleaning rust on surface of 7B04 aluminum alloy through nanosecond pulse laser
CN115837380A