Iron-aluminum slag resource utilization method and carbon-reduction full-chain waste lithium battery recycling method

Through steps such as water washing, acid leaching, sulfide precipitation and phosphoric acid treatment, the problem of complex iron and aluminum slag composition in lithium battery recycling is solved, efficient separation and high-purity recovery of nickel, cobalt, manganese, aluminum and iron are achieved, reducing processing costs. Improved the economic benefits of lithium battery recycling.

CN118754072AActive Publication Date: 2024-10-11HUNAN BRUNP RECYCLING TECH CO LTD +1

Patent Information

Application Number
CN202410839606.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

In the existing lithium battery recycling process, iron-aluminum slag has complex composition, and nickel, cobalt, manganese, iron and aluminum are mixed together and difficult to separate, resulting in complicated resource utilization, low recycling value, and disposal as hazardous waste with high costs, resulting in nickel, cobalt and manganese metal. losses and environmental stress.

Method used

Remove soluble impurities through water washing, acid leaching reaction and adding reducing agent to reduce ferric iron to divalent iron, then use sulfide to selectively precipitate nickel, cobalt and manganese, alkaline reagent precipitation to recover aluminum, and remove calcium and magnesium through step-by-step phosphoric acid treatment impurities, and finally prepare high-purity iron phosphate to achieve the separation of nickel, cobalt, manganese, aluminum and iron.

Benefits of technology

It improves the recovery rate and product purity, reduces processing costs, realizes efficient resource utilization of iron and aluminum slag, reduces the loss of nickel, cobalt and manganese metal, and improves the economic benefits of lithium battery recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754072A_ABST
    Figure CN118754072A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of resource utilization, and discloses an iron-aluminum slag resource utilization method and a carbon-reduction full-chain waste lithium battery recycling method. The iron and aluminum slag resource utilization method comprises the steps that iron and aluminum slag is washed, water is added into washed slag for pulping, then acid and a reducing agent are added for an acid leaching reaction, and leachate is obtained; sulfide is added into the lixivium, the pH is adjusted, nickel, cobalt and manganese removal reaction is carried out, and a nickel, cobalt and manganese removal solution is obtained; adding an alkali reagent into the nickel-cobalt-manganese-removed solution to carry out aluminum precipitation reaction to obtain an aluminum hydroxide product and an aluminum-removed solution; and adding first phosphoric acid into the aluminum-removed solution to remove calcium and magnesium, carrying out solid-liquid separation after the reaction is completed, adding second phosphoric acid and an oxidant into the obtained impurity-removed solution to carry out a synthetic reaction, and obtaining an iron phosphate product after the reaction is completed. According to the method, nickel, cobalt, manganese, aluminum and iron can be separated, corresponding products are obtained, the steps are high in separation recovery rate and purity, and production benefits can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource utilization, and in particular to a method for resource utilization of iron-aluminum slag and a method for recycling waste lithium batteries with a full carbon reduction chain. Background Art

[0002] At present, the lithium-ion battery industry is accelerating the transformation from "grey manufacturing" to "green manufacturing". In the critical period of focusing on carbon reduction and promoting the comprehensive green transformation of economic and social development, the lithium-ion battery industry is a key area for pollution reduction and carbon reduction.

[0003] With the rapid development of electric vehicles and energy storage, the market demand for lithium batteries continues to grow and the market size continues to expand. In terms of technology, the energy density of lithium batteries continues to increase, and the charging speed is also accelerating, which makes it possible for lithium batteries to be widely used in electric vehicles, smart phones, tablets and other fields. Among them, lithium batteries are most widely used in new energy vehicles. However, since the average service life of lithium batteries is 4 to 6 years, retired lithium batteries contain metals such as nickel, cobalt, manganese, lithium and copper. If they are not recycled, it will not only cause waste of resources, but also bring great pressure to the environment, which is not conducive to carbon reduction in the industrial chain and resource utilization of waste gas. Therefore, the recycling of retired lithium batteries has become an urgent problem to be solved. At present, the mainstream process for recycling retired lithium batteries is to discharge, disassemble, crush and sort lithium batteries to obtain black powder, copper slag, aluminum slag, diaphragm, etc., and then add acid and reducing agent to the black powder to leach it to obtain a solution containing nickel, cobalt, manganese, lithium, copper and aluminum and graphite slag. Iron powder is added to the solution to remove copper to obtain sponge copper and copper-removed liquid. Oxidant and alkaline reagent are added to the copper-removed liquid to remove iron and aluminum to obtain iron-removed aluminum liquid and iron-aluminum slag. After iron and aluminum are removed, the liquid is extracted to recover nickel, cobalt, manganese and lithium metals. When adding alkaline reagents to remove iron and aluminum, a part of nickel, cobalt and manganese metals will be precipitated together, resulting in 1 to 3 wt% nickel, cobalt and manganese in the iron-aluminum slag. In addition, since iron and aluminum are mixed together in the iron-aluminum slag, it is difficult to use iron and aluminum. In addition, since nickel and cobalt exceed the standard, the iron-aluminum slag produced by lithium battery recycling is generally treated as hazardous waste. This not only leads to the loss of high-value nickel, cobalt and manganese, but also iron and aluminum cannot be used, and the cost of hazardous waste treatment is high. Therefore, it is necessary to carry out the resource recovery process of iron-aluminum slag to expand the recyclability of lithium-ion battery recycled materials and achieve pollution reduction and carbon reduction.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a method for resource utilization of iron-aluminum slag and a method for recycling waste lithium batteries with a full chain of carbon reduction.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides a method for resource utilization of iron-aluminum slag, which comprises the following steps:

[0008] S1, washing the iron-aluminum slag with water to remove soluble impurities to obtain washed slag;

[0009] S2, adding water to the washed slag to make pulp, then adding acid and a reducing agent to carry out acid leaching reaction, and after the reaction is completed, solid-liquid separation is carried out to obtain a leachate and an insoluble slag;

[0010] S3, adding sulfide to the leachate and adjusting the pH to perform a nickel-cobalt-manganese removal reaction, and after the reaction is completed, performing solid-liquid separation to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag;

[0011] S4, adding an alkali reagent to the nickel-cobalt-manganese removal solution to carry out aluminum precipitation reaction, and after the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution;

[0012] S5, first adding the first phosphoric acid to the aluminum removal solution to remove calcium and magnesium, and after the reaction is completed, the solid-liquid separation is completed, and the second phosphoric acid and an oxidant are added to the obtained impurity removal liquid to carry out a synthesis reaction, and after the reaction is completed, an iron phosphate product is obtained.

[0013] In an optional embodiment, the ferroaluminum slag includes ferroaluminum slag obtained by hydrometallurgical removal of iron and aluminum from waste nickel-cobalt-manganese lithium batteries.

[0014] In an optional embodiment, the amount of the acid added is 1.0 to 1.5 times the theoretical amount of all metal elements in the water-washed slag; the amount of the reducing agent added is 1.0 to 1.5 times the theoretical amount of ferric iron;

[0015] And / or, the temperature of the acid leaching reaction is 40-70° C., and the reaction time is 5-12 hours;

[0016] and / or, the acid comprises one or more of sulfuric acid, hydrochloric acid and nitric acid;

[0017] And / or, the reducing agent includes one or more of iron powder, sodium sulfite and sodium thiosulfate.

[0018] In an optional embodiment, the amount of sulfide added is 1.0 to 3.0 times the theoretical amount of the reaction with nickel, cobalt and manganese;

[0019] And / or, the sulfide includes one or more of aluminum sulfide, ferrous sulfide, hydrogen sulfide and sodium sulfide;

[0020] And / or, the pH of the reaction system of the nickel, cobalt and manganese removal reaction is adjusted to 1.0-4.0 using sulfuric acid.

[0021] And / or, the nickel-cobalt-manganese slag is returned to the front end of the lithium battery hydrometallurgy for recycling.

[0022] In an optional embodiment, the alkaline reagent includes one of sodium hydroxide and sodium carbonate;

[0023] And / or, the reaction endpoint pH of the aluminum precipitation reaction is controlled at 4.0 to 7.0.

[0024] In an optional embodiment, the amount of the first phosphoric acid added is 1.1 to 3.0 times the theoretical amount for reacting with calcium and magnesium;

[0025] And / or, the reaction time after the first phosphoric acid is added is 1 to 3 hours.

[0026] In an optional embodiment, the amount of the second phosphoric acid added is 1.0 to 2.0 times the theoretical amount for reaction with iron;

[0027] And / or, the oxidant is hydrogen peroxide;

[0028] And / or, the reaction temperature of the synthesis reaction is 70-90° C., and the reaction time is 4.0-10 h.

[0029] In an optional embodiment, after the synthesis reaction is completed and before the ferric phosphate product is obtained, the reaction system is further aged, filtered, washed and dried;

[0030] Preferably, the aging time is 12 to 20 hours.

[0031] In a second aspect, the present invention provides a method for recycling waste lithium batteries with a full-chain carbon reduction, which includes the method for resource utilization of iron-aluminum slag as described in any of the aforementioned embodiments.

[0032] The present invention has the following beneficial effects:

[0033] The resource utilization method of the iron-aluminum slag provided by the present invention is to recycle the iron-aluminum slag obtained by the hydrometallurgical iron-aluminum removal process of waste lithium batteries. At present, the iron-aluminum slag produced in the lithium battery recycling process is basically treated as waste slag for brick burning due to the complex resource utilization process and low recycling value. The iron-aluminum slag has complex components, and nickel, cobalt, manganese, iron and aluminum are mixed together and are difficult to separate. In the present invention, during recovery, soluble impurities are first removed by water washing, and then the washed slag is acid-leached, and a reducing agent is added during the acid leaching process. The reducing agent can reduce the trivalent iron in the leachate to divalent iron to obtain a nickel-cobalt-manganese-iron-aluminum solution containing divalent iron. Subsequently, step-by-step precipitation is adopted to avoid interference from other metals when preparing the corresponding products. When precipitating nickel, cobalt and manganese, sulfide is added and the pH of the solution is controlled to selectively precipitate nickel, cobalt and manganese without introducing new impurities. After solid-liquid separation, an alkaline reagent is added to the nickel-cobalt-manganese removal solution to precipitate and recover aluminum. Since the pH of the divalent iron precipitation is greater than 6, the pH of the trivalent iron precipitation is 2.0-3.5, and the pH of the aluminum hydroxide precipitation is 3.2-5.5, the divalent iron will basically not precipitate when precipitating aluminum, thereby being able to prepare an aluminum hydroxide product with higher purity. Since the solution after aluminum precipitation contains calcium and magnesium ions, adding phosphoric acid in one step to prepare ferric phosphate will cause excessive calcium and magnesium impurities in the product. By adding phosphoric acid in steps, calcium and magnesium impurities are first removed, and then phosphoric acid and oxidant are added to prepare iron into high-purity ferric phosphate. Through a series of reasonable designs, nickel, cobalt, manganese, aluminum and iron can be separated to obtain corresponding products. At present, the recycling of 1 ton of metal from nickel-cobalt-manganese lithium batteries produces about 1.5 tons of iron-aluminum slag, and 1 ton of iron-aluminum slag requires 3,000 yuan as hazardous waste treatment. The method of the present invention can generate a benefit of 2,600 yuan / ton after recycling nickel, cobalt, manganese, iron and aluminum from iron-aluminum slag. Based on the annual processing of 10,000 tons of nickel-cobalt-manganese lithium batteries, the iron-aluminum slag resource method provided by the present invention is expected to bring a benefit of 39 million yuan. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 This is a process flow chart of the method for resource utilization of iron-aluminum slag provided by the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0037] See also Figure 1 The present invention provides a method for resource utilization of iron-aluminum slag, which comprises the following steps:

[0038] S1. Wash the iron-aluminum slag with water to remove soluble impurities and obtain washed slag.

[0039] S2, adding water to the washed slag to make pulp, then adding acid and a reducing agent to carry out acid leaching reaction, and after the reaction is completed, solid-liquid separation is carried out to obtain leachate and insoluble slag;

[0040] S3, adding sulfide to the leachate and adjusting the pH to perform a nickel-cobalt-manganese removal reaction, and after the reaction is completed, performing solid-liquid separation to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag;

[0041] S4, adding an alkali reagent to the nickel-cobalt-manganese removal solution to carry out an aluminum precipitation reaction, and after the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution;

[0042] S5. Firstly, the aluminum removal solution is added with the first phosphoric acid to remove calcium and magnesium. After the reaction is completed, the solid and liquid are separated. The second phosphoric acid and the oxidant are added to the obtained impurity removal liquid to carry out a synthesis reaction. After the reaction is completed, the iron phosphate product is obtained.

[0043] Traditionally, the iron-aluminum slag produced by the wet smelting of lithium batteries is treated as hazardous solid waste, with a processing cost of 3,000 yuan / ton, which not only causes the loss of nickel and cobalt metals, but also puts great pressure on the ecological environment. The present invention processes this part of the iron-aluminum slag, and can effectively separate and recover the nickel, cobalt, manganese, aluminum, and iron in the iron-aluminum slag. In the present invention, in view of the fact that nickel, cobalt, manganese, and iron and aluminum are difficult to separate in the iron-aluminum slag, the washed slag is first acid-leached, and a reducing agent is added during the acid-leaching process. The addition of the reducing agent can reduce the iron in the iron-aluminum slag to divalent iron, thereby avoiding the loss of iron caused by the subsequent aluminum precipitation process. Subsequently, nickel, cobalt, and manganese are selectively precipitated using sulfides, and aluminum is recovered by precipitation, and then phosphoric acid and an oxidant are added to obtain recovered iron. Nickel, cobalt, manganese, aluminum, and iron can be separated in this order to prepare corresponding products respectively. The above steps have high separation recovery rates and high purity, which can greatly improve production efficiency.

[0044] Specifically, the steps of the present invention are as follows:

[0045] S1. Wash with water.

[0046] The ferroaluminum slag is washed with water to remove soluble impurities to obtain washed slag. The ferroaluminum slag includes the ferroaluminum slag obtained by hydrometallurgical removal of iron and aluminum from waste nickel-cobalt-manganese lithium batteries. The water washing in the present invention can first remove soluble impurities, such as sodium, fluoride ions, etc., wherein the solid-liquid ratio of the water washing can be, for example, 1g:4-10ml. It should be noted that during the water washing process, some soluble calcium ions and magnesium ions may also be washed away, but due to the complex composition of the ferroaluminum slag, the subsequent leaching solution may still contain a small amount of calcium and magnesium impurities, which need to be removed again.

[0047] S2. Acid leaching reaction.

[0048] After the washed slag is slurried with water, acid and a reducing agent are added to carry out an acid leaching reaction, wherein the amount of acid added is 1.0 to 1.5 times the theoretical amount of reaction of all metal elements in the washed slag; the amount of reducing agent added is 1.0 to 1.5 times the theoretical amount of reaction of trivalent iron; the temperature of the acid leaching reaction is 40 to 70°C, and the reaction time is 5 to 12 hours; after the reaction is completed, solid-liquid separation is performed to obtain a leachate and an insoluble slag.

[0049] In some embodiments of the present invention, the acid includes but is not limited to one or more of sulfuric acid, hydrochloric acid and nitric acid; the reducing agent includes but is not limited to one or more of iron powder, sodium sulfite and sodium thiosulfate.

[0050] Taking sulfuric acid as the acid and iron powder as the reducing agent as an example, the reactions that occur during the acid leaching process are as follows:

[0051] NiCO3+H2SO4→NiSO4+H2O+CO2↑;

[0052] CoCO3+H2SO4→CoSO4+H2O+CO2↑;

[0053] MnCO3+H2SO4→MnSO4+H2O+CO2↑;

[0054] 2Al(OH)3+3H2SO4→Al2(SO4)3+6H2O;

[0055] Na2Al6(SO4)4.·(OH) 12 +6H2SO4→3Al2(SO4)3+Na2SO4+12H2O;

[0056] 2Fe(OH)3+3H2SO4→Fe2(SO4)3+6H2O;

[0057] Na2Fe6(SO4)4·(OH) 12 +6H2SO4→3Fe2(SO4)3+Na2SO4+12H2O;

[0058] Fe2(SO4)3+Fe→3FeSO4.

[0059] In the present invention, a reducing agent is added during the acid leaching process, so that the iron in the iron-aluminum slag can be reduced to divalent iron, thereby avoiding the loss of iron caused by the subsequent aluminum precipitation process.

[0060] S3, nickel, cobalt and manganese removal reaction.

[0061] Sulfide is added to the leachate, and the amount of sulfide added is 1.0 to 3.0 times the theoretical amount of the nickel, cobalt and manganese reaction. Sulfuric acid is used to adjust the pH to 1.0 to 4.0 to carry out the nickel, cobalt and manganese removal reaction. After the reaction is completed, the solid and liquid are separated to obtain a nickel, cobalt and manganese removal solution and a nickel, cobalt and manganese slag. The nickel, cobalt and manganese slag is returned to the front end of the lithium battery wet smelting for recycling.

[0062] In some embodiments of the present invention, the sulfide includes, but is not limited to, one or more of aluminum sulfide, ferrous sulfide, hydrogen sulfide and sodium sulfide.

[0063] In the present invention, sulfide is used as a precipitant to selectively precipitate nickel, cobalt and manganese in the leachate, and is removed by filtering. By first removing nickel, cobalt and manganese, the subsequent recovery rate and recovery purity of aluminum and iron can be effectively improved. Among them, the sulfide is preferably aluminum sulfide and ferrous sulfide. The use of ferrous sulfide and aluminum sulfide to remove nickel, cobalt and manganese can not introduce new impurities, and the cost is relatively low. When the sulfide is sodium sulfide, the introduced sodium can be removed by washing with water.

[0064] S4, aluminum precipitation reaction.

[0065] The nickel-cobalt-manganese removal solution is added with an alkaline reagent to carry out an aluminum precipitation reaction. The alkaline reagent includes but is not limited to one of sodium hydroxide and sodium carbonate. The reaction end point pH of the aluminum precipitation reaction is controlled at 4.0-7.0. After the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution.

[0066] Since aluminum hydroxide is insoluble in water and alcohol but soluble in inorganic acid and alkaline solutions, in step S3, the nickel-cobalt-manganese solution is acidic. At this time, the aluminum ions are in a dissolved state. In the present invention, an alkaline reagent is added to adjust the pH of the reaction system so that aluminum hydroxide is gradually precipitated, thereby effectively separating the aluminum hydroxide.

[0067] S5. Synthesis reaction.

[0068] The aluminum removal solution is first added with the first phosphoric acid to remove calcium and magnesium. The amount of the first phosphoric acid added is 1.1 to 3.0 times the theoretical amount of the reaction with calcium and magnesium. The reaction time after the first phosphoric acid is added is 1 to 3 hours. After the reaction is completed, the solid and liquid are separated. The second phosphoric acid and an oxidant (such as 27.5% hydrogen peroxide) are added to the obtained impurity removal liquid for synthesis reaction. The amount of the second phosphoric acid added is 1.0 to 2.0 times the theoretical amount of the reaction with iron. The reaction temperature is 70 to 90°C, and the reaction time is 4.0 to 10 hours. After the reaction is completed, the iron phosphate product is obtained.

[0069] In the present invention, the composition of the iron-aluminum slag is relatively complex, and the solution after leaching contains a small amount of calcium and magnesium impurities. By adding phosphoric acid step by step, the calcium and magnesium impurities in the solution are first precipitated into calcium phosphate and magnesium phosphate. After solid-liquid separation, phosphoric acid and an oxidant are added to the solution to prepare a high-purity iron phosphate product.

[0070] S6, aging, filtering, washing and drying.

[0071] The reaction system of the synthesis reaction is aged for 12 to 20 hours, filtered, washed and dried.

[0072] In addition, the present invention also provides a carbon reduction full-chain waste lithium battery recycling method, which includes the above-mentioned iron-aluminum slag resource utilization method. Traditionally, the iron-aluminum slag produced by lithium battery hydrometallurgy is treated as hazardous solid waste, with a treatment cost of 3,000 yuan / ton, which not only causes the loss of nickel and cobalt metals, but also puts great pressure on the ecological environment. The present invention treats this part of the iron-aluminum slag, which can effectively separate and recover the nickel, cobalt, manganese, aluminum, and iron in the iron-aluminum slag, with high recovery rate and high purity, which can greatly improve production efficiency.

[0073] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0074] Example 1

[0075] This embodiment provides a method for resource utilization of iron-aluminum slag, which comprises the following steps:

[0076] S1. Take 500g of iron-aluminum slag obtained by the wet smelting and iron-aluminum removal process of waste lithium batteries and wash it with water to remove soluble sodium and fluoride ions. The washed slag is used for the next step, and the washing water is sent to the wastewater workshop for treatment.

[0077] The composition and content of iron-aluminum slag can be found in Table 1:

[0078] Table 1. Statistics of iron and aluminum slag composition content / %

[0079] Ni Co Mn Al Fe Na F Ca Mg S, O, C, H 1.5 0.1 0.06 12.8 16.9 7.6 3.2 0.32 0.17 >50

[0080] S2. After the washed slag obtained in step S1 is slurried with water, sulfuric acid in an amount 1.1 times the theoretical amount to react with all metal elements in the washed slag and iron powder in an amount 1.2 times the theoretical amount to react with trivalent iron in the washed slag are added to react, the reaction temperature is controlled at 60° C. After reacting for 5 hours, the solid and liquid are separated to obtain a leachate and an insoluble slag.

[0081] S3. The leaching solution obtained in step S2 is added with ferrous sulfide in an amount 1.5 times the theoretical amount for reacting with nickel, cobalt and manganese, and the pH value of the solution is adjusted to 1.0 with sulfuric acid. After the reaction, the solid-liquid separation is performed to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag. The nickel-cobalt-manganese slag is returned to the front end of the lithium battery wet smelting process for recovery treatment. The recovery rates of nickel, cobalt and manganese are calculated to be 99%, 98% and 97%, respectively.

[0082] S4. The nickel-cobalt-manganese removal solution obtained in step S3 is added to a 32% sodium hydroxide solution for reaction. The pH value is controlled to be stable at 6.0 at the reaction end point. After the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution. The aluminum hydroxide is washed with water and dried to obtain an aluminum hydroxide product. The aluminum hydroxide product is tested to have an Al content of 33.5% and a purity of 97%.

[0083] Table 2. Statistical table of aluminum hydroxide content / %

[0084] Ni Co Mn Al Fe F 0.0001 0.005 0.008 33.5 0.002 1.5

[0085] S5. The aluminum removal solution obtained in step S4 is first added with 3.0 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react for 2 hours. After the reaction is completed, the solid-liquid separation is performed, and the obtained solution is further added with 1.1 times the theoretical amount of phosphoric acid that reacts with iron and 1.2 times 27.5% hydrogen peroxide to react at a reaction temperature of 85°C. After reacting for 8 hours, it is aged for 12 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is greater than 99% after testing.

[0086] Table 3. Iron phosphate content / %

[0087] Fe P Al Na Ni Co Mn Ca Mg F 36.8 20.4 0.0001 0.001 0.0001 0.0001 0.0001 0.0001 0.0001 0.0001

[0088] Example 2

[0089] A method for resource utilization of iron-aluminum slag comprises the following specific steps:

[0090] S1. Take 200g of iron-aluminum slag obtained by the wet smelting and iron-aluminum removal process of waste lithium batteries and wash it with water to remove soluble sodium and fluoride ions. The washed slag is used for the next step, and the washing water is sent to the wastewater workshop for treatment.

[0091] Table 4. Iron and aluminum slag composition content / %

[0092] Ni Co Mn Al Fe Na F Ca Mg S, O, C, H 1.7 0.8 0.3 15.8 11.9 6.6 2.7 0.15 0.08 >50

[0093] S2. After the washed slag obtained in step S1 is slurried with water, sulfuric acid in an amount 1.1 times the theoretical amount to react with all metal elements in the washed slag and sodium sulfite in an amount 1.1 times the theoretical amount to react with trivalent iron in the washed slag are added to react, the reaction temperature is controlled at 50° C. After reacting for 12 hours, the solid and liquid are separated to obtain a leachate and an insoluble slag.

[0094] S3. The leaching solution obtained in step S2 is added with 2.0 times the theoretical amount of aluminum sulfide that can react with nickel, cobalt and manganese, and the pH value of the solution is adjusted to 3.0 with sulfuric acid. After the reaction, the solid-liquid separation is performed to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag. The nickel-cobalt-manganese slag is returned to the front end of the lithium battery wet smelting process for recovery treatment. The recovery rates of nickel, cobalt and manganese are calculated and tested to be 99%, 99% and 98%, respectively.

[0095] S4. Add the nickel-cobalt-manganese removal solution obtained in step S3 into 20% sodium carbonate solution for reaction. The pH value is controlled to be stable at 6.5 at the reaction end point. After the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution. The aluminum hydroxide is washed with water and dried to obtain an aluminum hydroxide product. The aluminum hydroxide content is 33.7% and the purity of the aluminum hydroxide is 97%.

[0096] Table 5. Aluminum hydroxide content / %

[0097] Ni Co Mn Al Fe F 0.0001 0.0002 0.0001 33.7 0.004 1.2

[0098] S5. The aluminum removal solution obtained in step S4 is first added with 1.5 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react for 2 hours. After the reaction is completed, the solid-liquid separation is performed, and the obtained solution is further added with 1.1 times the theoretical amount of phosphoric acid that reacts with iron and 1.1 times 27.5% hydrogen peroxide to react at a reaction temperature of 90° C. After reacting for 6 hours, it is aged for 20 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is greater than 99% after testing.

[0099] Table 6. Iron phosphate content / %

[0100] Fe P Al Na Ni Co Mn Ca Mg F 36.9 20.3 0.0001 0.0012 0.0001 0.0001 0.0001 0.0001 0.0001 0.0001

[0101] Example 3

[0102] A method for resource utilization of iron-aluminum slag comprises the following specific steps:

[0103] S1. Take 1000g of iron-aluminum slag obtained by the wet smelting and iron-aluminum removal process of waste lithium batteries and wash it with water to remove soluble sodium and fluoride ions. The washed slag is used for the next step, and the washing water is sent to the wastewater workshop for treatment.

[0104] The composition and content of iron-aluminum slag can be found in Table 7:

[0105] Table 7. Statistics of iron and aluminum slag composition content / %

[0106] Ni Co Mn Al Fe Na F Ca Mg S, O, C, H 2.3 1.1 0.3 10.8 18.3 5.7 4.1 0.25 0.19 >50

[0107] S2. After the washed slag obtained in step S1 is slurried with water, sulfuric acid in an amount 1.1 times the theoretical amount to react with all metal elements in the washed slag and iron powder in an amount 1.2 times the theoretical amount to react with trivalent iron in the washed slag are added to react, the reaction temperature is controlled at 60° C. After reacting for 6 hours, the solid and liquid are separated to obtain a leachate and an insoluble slag.

[0108] S3. The leaching solution obtained in step S2 is added with ferrous sulfide in an amount 1.2 times the theoretical amount for reacting with nickel, cobalt and manganese, and the pH value of the solution is adjusted to 2.0 with sulfuric acid. After the reaction, the solid-liquid separation is performed to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag. The nickel-cobalt-manganese slag is returned to the front end of the lithium battery wet smelting process for recovery treatment. The recovery rates of nickel, cobalt and manganese are calculated to be 99%, 97% and 96%, respectively.

[0109] S4. Add the nickel-cobalt-manganese removal solution obtained in step S3 into 32% sodium hydroxide solution for reaction. The pH value is controlled to be stable at 6.0 at the reaction end point. After the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution. The aluminum hydroxide is washed with water and dried to obtain an aluminum hydroxide product. The Al content is 32.9% and the aluminum removal purity of the aluminum hydroxide is 95%.

[0110] Table 8. Aluminum hydroxide content / %

[0111] Ni Co Mn Al Fe F 0.0005 0.015 0.08 32.9 0.005 1.6

[0112] S5. The aluminum removal solution obtained in step S4 is first added with 2.0 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react for 2 hours. After the reaction is completed, the solid-liquid separation is performed. The obtained solution is first added with 1.2 times the theoretical amount of phosphoric acid that reacts with iron and 1.5 times 27.5% hydrogen peroxide to react. The reaction temperature is 90° C. After reacting for 5 hours, it is aged for 15 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is greater than 99% after testing.

[0113] Table 9. Iron phosphate content / %

[0114] Fe P Al Na Ni Co Mn Ca Mg F 36.9 20.4 0.0001 0.0015 0.0001 0.0001 0.0001 0.0001 0.0001 0.0001

[0115] Comparative Example 1

[0116] A method for resource utilization of iron-aluminum slag, which is basically the same as Example 1, the main difference is that in this comparative example, aluminum is first precipitated, then iron phosphate is synthesized, and finally nickel, cobalt and manganese are precipitated and recovered, which includes the following specific steps:

[0117] S1 and S2 are the same as those in Example 1.

[0118] S3. The leachate obtained in step S2 of Example 1 is added with 20% sodium carbonate solution to react. The pH value is controlled to be stable at 5.5 at the reaction end point. After the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution. The aluminum hydroxide is washed with water and dried to obtain an aluminum hydroxide product. The Al content is 31.5% and the purity of the aluminum hydroxide is 91%.

[0119] Table 10. Aluminum hydroxide content / %

[0120] Ni Co Mn Al Fe F 0.66 0.25 0.016 31.5 0.001 0.15

[0121] S4. The aluminum removal solution obtained in step S3 is first added with 3.0 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react for 2 hours. After the reaction is completed, the solid-liquid separation is performed, and the obtained solution is further added with 1.1 times the theoretical amount of phosphoric acid that reacts with iron and 1.2 times 27.5% hydrogen peroxide to react at a reaction temperature of 85°C. After reacting for 8 hours, it is aged for 12 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is 97% after testing.

[0122] Table 11 Iron phosphate content / %

[0123] Fe P Al Na Ni Co Mn Ca Mg F 35.8 19.8 0.0026 0.001 0.0042 0.0015 0.0001 0.0001 0.0001 0.0001

[0124] S5. The filtrate is then added with 20% sodium hydroxide solution to recover the remaining nickel, cobalt and manganese metals through precipitation. After analysis and detection, the recovery rates of nickel, cobalt and manganese metals are 75%, 81% and 92% respectively.

[0125] From the data comparison between Comparative Example 1 and Example 1, it can be seen that the recovery rates of nickel, cobalt and manganese in Example 1 are 99%, 98% and 97% respectively, and the purity of the output aluminum hydroxide is 97% and the purity of iron phosphate is greater than 99%. In Comparative Example 1, since nickel, cobalt and manganese are not preferentially recovered, not only the purity of aluminum hydroxide and iron phosphate products is reduced, the content of nickel, cobalt and manganese in aluminum hydroxide is significantly higher than that in Example 1, the nickel content in the iron phosphate product is significantly higher than that in Example 1, and the recovery rate of nickel, cobalt and manganese is significantly reduced.

[0126] Comparative Example 2

[0127] This comparative example is basically the same as comparative example 1, except that in this comparative example, aluminum is first precipitated, then nickel, cobalt and manganese are precipitated, and finally iron phosphate is synthesized, which includes the following specific steps:

[0128] S1, S2 and S3 are the same as Comparative Example 1.

[0129] S4. The aluminum removal solution obtained in step S3 is added with ferrous sulfide in an amount 1.5 times the theoretical amount for the reaction with nickel, cobalt and manganese, and sulfuric acid is used to adjust the pH value of the solution to 3.0. After the reaction, the solid-liquid separation is performed to obtain a nickel, cobalt and manganese removal solution and a nickel, cobalt and manganese slag. The nickel, cobalt and manganese slag is returned to the front end of the lithium battery wet smelting process for recovery and treatment. The recovery rates of nickel, cobalt and manganese are calculated to be 84%, 91% and 95%, respectively.

[0130] S5. The nickel-cobalt-manganese removal solution obtained in step S4 is first added with 1.5 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react for 2 hours. After the reaction is completed, the solid-liquid separation is performed, and the obtained solution is further added with 1.1 times the theoretical amount of phosphoric acid that reacts with iron and 1.1 times 27.5% hydrogen peroxide to react at a reaction temperature of 90° C. After reacting for 6 hours, it is aged for 20 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is greater than 98% after testing.

[0131] Table 12. Iron phosphate content / %

[0132] Fe P Al Na Ni Co Mn Ca Mg F 36.2 20.0 0.0001 0.023 0.0001 0.0001 0.002 0.0001 0.0001 0.0001

[0133] From the data comparison of Comparative Example 1, Comparative Example 2 and Example 1, it can be seen that in Comparative Example 2, since aluminum is precipitated before recovering nickel, cobalt and manganese, the purity of aluminum hydroxide is significantly lower than that in Example 1. Nickel, cobalt and manganese are recovered after aluminum precipitation, which results in a nickel, cobalt and manganese recovery rate that is significantly lower than that in Example 1, but slightly higher than that in Comparative Example 1, and the purity of the ferric phosphate product is also slightly higher than that in Comparative Example 1, but still significantly lower than that in Example 1.

[0134] Comparative Example 3

[0135] A method for resource utilization of iron-aluminum slag is basically the same as Example 2, the main difference being that in this comparative example, no reducing agent is added during the acid leaching process, but oxidative leaching is performed.

[0136] It includes the following specific steps:

[0137] S1. Same as Example 2.

[0138] S2. Take the washed slag obtained in S1 in Example 2, add water to make pulp, then add 1.1 times the theoretical amount of sulfuric acid and 1.2 times the theoretical amount of hydrogen peroxide to react, control the reaction temperature to 50°C, react for 12 hours, separate the solid and liquid, and obtain the leaching solution and insoluble slag.

[0139] S3 was carried out with reference to Example 2, wherein the recovery rates of nickel, cobalt and manganese in S3 were 99%, 98% and 98% respectively.

[0140] S4 is carried out with reference to Example 2, wherein the Al content in the aluminum hydroxide product in S4 is detected to be 15.6%, and the purity of aluminum hydroxide after aluminum precipitation is 54%. Since trivalent iron is easier to precipitate than aluminum ions, a mixed product of iron and aluminum is obtained in this step, and there is almost no trivalent iron in the solution after aluminum precipitation.

[0141] Table 13. Aluminum hydroxide content / %

[0142] Ni Co Mn Al Fe F 0.0001 0.004 0.008 15.6 16.3 1.4

[0143] From the data comparison of Comparative Example 3 and Example 2, it can be seen that in Comparative Example 3, hydrogen peroxide is used as a reducing agent during acid leaching, resulting in trivalent iron in the leachate. Since the precipitation pH of trivalent iron is lower than that of aluminum ions, trivalent iron in the solution will precipitate together when aluminum ions are precipitated, and the obtained product is a mixture of iron and aluminum, which cannot effectively separate iron and aluminum.

[0144] Comparative Example 4

[0145] This comparative example is basically the same as Example 2, except that in step S3, resin adsorption is used to remove nickel, cobalt and manganese, which includes the following specific steps:

[0146] S1 and S2 are the same as those in Example 2.

[0147] S3, the leachate obtained in step S2 is adsorbed by resin, two resin columns are connected in series, and the Ni, Co, and Mn contents of the tail column outlet liquid are controlled to be less than 2 mg / L to obtain a solution after adsorbing nickel, cobalt, and manganese. The saturated adsorption resin is analyzed by 3.0 mol / L sulfuric acid to obtain a sulfate solution enriched in nickel and cobalt. The recovery rates of nickel, cobalt, and manganese are all greater than 99%. The nickel, cobalt, and manganese sulfate solution is returned to the front end of the hydrometallurgical process for recovery and treatment.

[0148] S4 is carried out with reference to Example 2, wherein the Al content in the aluminum hydroxide product in S4 is detected to be 33.6%, and the purity of the aluminum hydroxide after removing aluminum is 97%.

[0149] Table 14. Aluminum hydroxide content / %

[0150] Ni Co Mn Al Fe F 0.0001 0.0001 0.0002 33.6 0.003 1.3

[0151] S5 is carried out with reference to Example 2, wherein the purity of the ferric phosphate product in S3 is greater than 99%.

[0152] Table 15. Iron phosphate content / %

[0153] Fe P Al Na Ni Co Mn Ca Mg F 36.8 20.2 0.0001 0.0011 0.0001 0.0001 0.0001 0.0001 0.0002 0.0001

[0154] From the data comparison of Comparative Example 4 and Example 2, it can be seen that in Comparative Example 4, resin is used to adsorb nickel, cobalt and manganese. The purity of the aluminum hydroxide and ferric phosphate products prepared from the solution after adsorbing nickel, cobalt and manganese is almost the same as that of Example 2, and the product purity is relatively high. However, when using resin adsorption to remove nickel, cobalt and manganese, since there is currently no single resin that can adsorb nickel, cobalt and manganese at the same time, two or more resin combinations are required to remove nickel, cobalt and manganese in the solution to within the qualified range. In addition, the iron-aluminum slag leachate contains calcium, and calcium sulfate has the risk of being deposited on the resin surface, thereby affecting the resin performance. In addition, the resin needs to be analyzed and regenerated after adsorption, which leads to the generation of wastewater. Taking all factors into consideration, the resin is not only cumbersome in the process of removing nickel, cobalt and manganese, but also relatively high in cost, and the resin performance has the risk of deterioration. The present invention uses ferrous sulfide and aluminum sulfide to remove nickel, cobalt and manganese without introducing new impurities, and the cost is relatively low.

[0155] Comparative Example 5

[0156] This comparative example is basically the same as Example 2, except that in this comparative example, iron phosphate is first synthesized and then aluminum is precipitated, which includes the following specific steps:

[0157] S1, S2 and S3 are the same as those in Example 2.

[0158] S4. The nickel-cobalt-manganese removal solution obtained in step S3 is first added with 1.5 times the theoretical amount of phosphoric acid that reacts with calcium and magnesium to react. After the reaction is completed, the solid-liquid separation is performed, and the obtained solution is further added with 1.1 times the theoretical amount of phosphoric acid that reacts with iron and 1.1 times 27.5% hydrogen peroxide to react. The reaction temperature is 90° C. After reacting for 6 hours, it is aged for 20 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate is 48% after testing.

[0159] Table 16. Iron phosphate content / %

[0160] Fe P Al Na Ni Co Mn Ca Mg F 16.4 9.0 13.5 0.001 0.0001 0.0001 0.0002 0.0001 0.0001 0.002

[0161] S5. Add 20% sodium carbonate solution to the filtrate of step S4 to react, and control the pH value to be stable at 6.5 at the reaction end point. After the reaction is completed, perform solid-liquid separation to obtain an aluminum hydroxide product and a solution. The aluminum hydroxide is washed with water and dried to obtain an aluminum hydroxide product. The aluminum hydroxide content is 12.1% after testing, and the purity of the aluminum hydroxide is 42%.

[0162] Table 17. Aluminum hydroxide content / %

[0163] Ni Co Mn Al Fe F 0.0001 0.0002 0.0001 12.1 9.6 0.002

[0164] From the data comparison between Comparative Example 5 and Example 2, it can be seen that in Comparative Example 5, iron phosphate is synthesized first and then aluminum is precipitated. Since aluminum phosphate Ksp = 6.3×10 -19, iron phosphate dihydrate Ksp = 9.9 × 10 -19 The solubility product of the two is close, which will result in a decrease in the purity of iron phosphate when phosphate precipitation is added, because aluminum will also react with part of the phosphoric acid to form aluminum phosphate.

[0165] Comparative Example 6

[0166] This comparative example is basically the same as Example 3, except that in this comparative example, step S5 uses sodium fluoride to remove calcium and magnesium, and specifically includes the following steps.

[0167] The aluminum removal solution obtained in step S4 of Example 3 was first added with 3.0 times the theoretical amount of sodium fluoride to react with calcium and magnesium for reaction. After the reaction, the solid-liquid separation was performed. The obtained solution was first added with 1.2 times the theoretical amount of phosphoric acid and 1.5 times 27.5% hydrogen peroxide to react with iron. The reaction temperature was 90° C. After reacting for 5 hours, it was aged for 15 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate was greater than 98% after testing.

[0168] Table 18. Iron phosphate content / %

[0169] Fe P Al Na Ni Co Mn Ca Mg F 36.2 19.6 0.0001 0.0011 0.0001 0.0001 0.0001 0.0001 0.0001 0.018

[0170] From the comparison of the data of Comparative Example 6 and Example 3, it can be seen that in Comparative Example 6, sodium fluoride is used to remove calcium and magnesium. Although the obtained iron phosphate has a high purity and very low calcium and magnesium impurities, the fluorine content is as high as 180 ppm.

[0171] Comparative Example 7

[0172] This comparative example is basically the same as Example 3, except that in step S5 of this comparative example, all phosphoric acid is added at once, and phosphoric acid is not added step by step. Specifically, it includes the following steps.

[0173] The aluminum removal solution obtained in step S4 of Example 3 was added with 1.3 times the theoretical amount of phosphoric acid and 1.5 times 27.5% hydrogen peroxide to react with iron. The reaction temperature was 90°C. After reacting for 5 hours, the mixture was aged for 15 hours, and then filtered, washed, and dried to obtain an iron phosphate product. The purity of the iron phosphate was greater than 98%.

[0174] Table 19. Iron phosphate content / %

[0175] Fe P Al Na Ni Co Mn Ca Mg F 35.8 19.2 0.0001 0.0011 0.0001 0.0001 0.0001 0.015 0.0087 0.0001

[0176] From the comparison of the data of Comparative Example 7 and Example 3, it can be seen that in Comparative Example 7, phosphoric acid is directly added. At this time, the phosphoric acid reacts with the calcium, magnesium and iron in the aluminum removal solution to form a precipitate, resulting in the final ferric phosphate product having a significantly higher calcium and magnesium content than Example 3.

[0177] Comparative Example 8

[0178] This comparative example is basically the same as Example 3, except that the recycled raw materials in this comparative example are different. In this comparative example, the black powder obtained by disassembling the waste lithium batteries is directly used as the raw material, and the recycling is carried out according to the method of Example 3, wherein the components of the waste lithium batteries include nickel-cobalt-manganese lithium batteries or lithium iron phosphate.

[0179] Table 20. Statistics of black powder content of nickel-cobalt-manganese lithium batteries / %

[0180] Ni Co Mn Li Cu Al F Fe O, C 24.2 3.6 7.3 4.2 2.5 1.9 2.3 0.2 >50

[0181] Table 21. Statistics of black powder content in lithium iron phosphate batteries / %

[0182] Fe P Li Cu Al F Fe O, C 32.5 18.1 4.0 2.6 2.3 1.8 0.2 >50

[0183] Table 22. Aluminum hydroxide content / % (prepared from nickel-cobalt-manganese lithium battery as raw material)

[0184] Ni Co Mn Li Al Fe F 6.3 3.5 1.6 1.2 16.3 0.005 1.6

[0185] Table 23. Aluminum hydroxide content / % (prepared with lithium iron phosphate battery as raw material)

[0186]

[0187]

[0188] Table 24. Iron phosphate content / % (prepared with nickel-cobalt-manganese lithium battery as raw material)

[0189] Fe P Al Na Ni Co Mn Ca Mg F 31.57 17.47 0.0001 0.25 0.52 0.21 0.019 0.0001 0.0001 0.018

[0190] Table 25. Iron phosphate content / % (prepared with lithium iron phosphate battery as raw material)

[0191] Fe P Al Na Ca Mg S F 33.8 18.7 0.0001 0.36 0.0001 0.0001 0.69 0.018

[0192] In Comparative Example 8, the purities of aluminum hydroxide obtained using nickel-cobalt-manganese lithium battery black powder and lithium iron phosphate black powder as raw materials are 56% and 44%, respectively, and the purities of iron phosphate are 91% and 85%, respectively. Compared with the data in Example 3, it can be seen that the method provided by the present invention is designed for the iron-aluminum slag obtained by the wet smelting and iron-aluminum removal process of waste lithium batteries, which is directly used to recycle waste lithium batteries. Due to the high metal content in lithium batteries, it is difficult to completely remove impurities during impurity removal, and the addition of a large amount of impurity removal agents will introduce other impurities, resulting in a high impurity content in the prepared product.

[0193] In summary, the resource utilization method of the iron-aluminum slag provided by the present invention is to recycle the iron-aluminum slag obtained by the hydrometallurgical iron-aluminum removal process of waste lithium batteries. At present, the iron-aluminum slag produced in the lithium battery recycling process is basically treated as waste slag for brick burning due to its complex resource utilization process and low recycling value. The iron-aluminum slag has complex components, and nickel, cobalt, manganese, iron, and aluminum are mixed together and are difficult to separate. In the present invention, during recovery, soluble impurities are first removed by water washing, and then the washed slag is acid-leached, and a reducing agent is added during the acid leaching process. The reducing agent can reduce the trivalent iron in the leachate to divalent iron to obtain a nickel-cobalt-manganese-iron-aluminum solution containing divalent iron. Subsequently, step-by-step precipitation is adopted to avoid interference from other metals when preparing the corresponding products. When precipitating nickel, cobalt and manganese, sulfide is added and the pH of the solution is controlled to selectively precipitate nickel, cobalt and manganese without introducing new impurities. After solid-liquid separation, an alkaline reagent is added to the nickel-cobalt-manganese removal solution to precipitate and recover aluminum. Since the pH of the divalent iron precipitation is greater than 6, the pH of the trivalent iron precipitation is 2.0-3.5, and the pH of the aluminum hydroxide precipitation is 3.2-5.5, the divalent iron will basically not precipitate when precipitating aluminum, thereby being able to prepare an aluminum hydroxide product with higher purity. Since the solution after aluminum precipitation contains calcium and magnesium ions, adding phosphoric acid in one step to prepare ferric phosphate will cause excessive calcium and magnesium impurities in the product. By adding phosphoric acid in steps, calcium and magnesium impurities are first removed, and then phosphoric acid and oxidant are added to prepare iron into high-purity ferric phosphate. Through a series of reasonable designs, nickel, cobalt, manganese, aluminum and iron can be separated to obtain corresponding products. At present, the recycling of 1 ton of metal from nickel-cobalt-manganese lithium batteries produces about 1.5 tons of iron-aluminum slag, and 1 ton of iron-aluminum slag requires 3,000 yuan as hazardous waste treatment. The method of the present invention can generate a benefit of 2,600 yuan / ton after recycling nickel, cobalt, manganese, iron and aluminum from iron-aluminum slag. Based on the annual processing of 10,000 tons of nickel-cobalt-manganese lithium batteries, the iron-aluminum slag resource method provided by the present invention is expected to bring a benefit of 39 million yuan.

[0194] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for resource utilization of iron and aluminum slag, characterized in that: It includes the following steps: S1, washing the iron-aluminum slag with water to remove soluble impurities to obtain washed slag; S2, adding water to the washed slag to make pulp, then adding acid and a reducing agent to carry out acid leaching reaction, and after the reaction is completed, solid-liquid separation is carried out to obtain a leachate and an insoluble slag; S3, adding sulfide to the leachate and adjusting the pH to perform a nickel-cobalt-manganese removal reaction, and after the reaction is completed, performing solid-liquid separation to obtain a nickel-cobalt-manganese removal solution and a nickel-cobalt-manganese slag; S4, adding an alkali reagent to the nickel-cobalt-manganese removal solution to carry out aluminum precipitation reaction, and after the reaction is completed, solid-liquid separation is performed to obtain an aluminum hydroxide product and an aluminum removal solution; S5, first adding the first phosphoric acid to the aluminum removal solution to remove calcium and magnesium, and after the reaction is completed, the solid-liquid separation is completed, and the second phosphoric acid and an oxidant are added to the obtained impurity removal liquid to carry out a synthesis reaction, and after the reaction is completed, an iron phosphate product is obtained.

2. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The iron-aluminum slag includes the iron-aluminum slag obtained by hydrometallurgical removal of iron and aluminum from waste nickel-cobalt-manganese lithium batteries.

3. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The amount of the acid added is 1.0 to 1.5 times the theoretical amount of all metal elements in the water-washed slag; the amount of the reducing agent added is 1.0 to 1.5 times the theoretical amount of ferric iron; And / or, the temperature of the acid leaching reaction is 40-70° C., and the reaction time is 5-12 hours.

4. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The acid includes one or more of sulfuric acid, hydrochloric acid and nitric acid; And / or, the reducing agent includes one or more of iron powder, sodium sulfite and sodium thiosulfate.

5. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The amount of sulfide added is 1.0 to 3.0 times the theoretical amount of the sulfide to react with nickel, cobalt and manganese; And / or, the sulfide includes one or more of aluminum sulfide, ferrous sulfide, hydrogen sulfide and sodium sulfide; And / or, the reaction system of the nickel, cobalt and manganese removal reaction is adjusted to pH 1.0 to 4.0 using sulfuric acid; And / or, the nickel-cobalt-manganese slag is returned to the front end of the lithium battery hydrometallurgy for recycling.

6. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The alkaline reagent includes one of sodium hydroxide and sodium carbonate; And / or, the reaction endpoint pH of the aluminum precipitation reaction is controlled at 4.0 to 7.

0.

7. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The amount of the first phosphoric acid added is 1.1 to 3.0 times the theoretical amount for reacting with calcium and magnesium; And / or, the reaction time after the first phosphoric acid is added is 1 to 3 hours.

8. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: The amount of the second phosphoric acid added is 1.0 to 2.0 times the theoretical amount for reaction with iron; And / or, the oxidant is hydrogen peroxide; And / or, the reaction temperature of the synthesis reaction is 70-90° C., and the reaction time is 4.0-10 h.

9. The method for resource utilization of iron-aluminum slag according to claim 1, characterized in that: After the synthesis reaction is completed, before the ferric phosphate product is obtained, the reaction system is subjected to aging, filtering, washing and drying treatments; Preferably, the aging time is 12 to 20 hours.

10. A method for recycling waste lithium batteries with a full carbon reduction chain, characterized in that: It includes the method for resource utilization of iron-aluminum slag as described in any one of claims 1-9.

Citation Information

Patent Citations

  • Comprehensive utilization method for iron-aluminum slag

    CN105506290A

  • Method for preparing battery-grade iron phosphate by utilizing positive electrode powder of waste lithium iron phosphate battery

    CN116177510A

  • Preparation method of battery-grade iron phosphate

    CN117003211A

  • Extracting and recovering metals from cathode active materials from li-ion batteries using sulfide minerals and chemicals

    WO2024130244A1

Cited By

  • Resource recycling method for waste residues containing nickel, cobalt, iron and aluminum