Method for preparing flame-retardant ammonium polyphosphate from raffinate acid
Flame-retardant ammonium polyphosphate is prepared by neutralizing the raffinate acid with ammonia and then polymerizing it with urea and phosphorus pentoxide, which solves the problems of high energy consumption in phosphoric acid preparation and insufficient utilization of raffinate acid, and achieves high efficiency, The production of environmentally friendly flame-retardant ammonium polyphosphate reduces production costs and improves the flame-retardant performance of the product.
Patent Information
- Application Number
- CN202410792641.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
The existing phosphoric acid preparation process has problems such as high energy consumption, dust and harmful gas generation, and it cannot effectively utilize the raffinate acid to prepare flame-retardant ammonium polyphosphate.
The MAP slurry is generated by neutralizing the raffinate acid with ammonia gas, and polymerizing it with urea and phosphorus pentoxide in a polymerization reactor, controlling the reaction conditions such as temperature, pressure and stirring frequency, and finally adding melamine as a sealing agent. Terminal agent to prepare flame retardant ammonium polyphosphate.
The preparation of flame-retardant ammonium polyphosphate with high yield, low energy consumption and environmental protection is achieved, which significantly reduces the production cost and improves the polymerization degree and flame retardant performance of the product.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a method for preparing flame-retardant ammonium polyphosphate using raffinate acid. Background Art
[0002] Flame retardants are a kind of auxiliary agent commonly used in polymer materials, mainly halogen flame retardants, phosphorus flame retardants, and metal hydroxide flame retardants. Halogen flame retardants have high flame retardant efficiency, but they will produce toxic and polluting compounds when burning, which will cause great harm to the human body and the environment. With the continuous improvement of people's environmental awareness, halogen flame retardants are gradually being eliminated. Phosphorus flame retardants have the characteristics of non-toxicity, halogen-free, smoke suppression, high flame retardant efficiency and environmental friendliness. In addition, phosphorus has the characteristics of production degradation, and will not encounter environmental persistence and bioaccumulation problems during use. Ammonium polyphosphate (APP), as an inorganic phosphorus flame retardant, has the characteristics of non-toxicity, halogen-free, smoke suppression, good flame retardant effect and environmental friendliness. It is widely used in plastics such as polypropylene, polyurethane, epoxy resin, etc., and has broad application prospects.
[0003] Phosphoric acid production methods are mainly divided into wet and thermal methods, but the preparation of phosphoric acid by thermal phosphoric acid requires a lot of energy consumption, and the production process is accompanied by the generation of dust and harmful gases, which will cause harm to the human body and the environment. Wet phosphoric acid has become the main way to purify phosphoric acid in various countries, but the production process will produce raffinate acid containing high concentrations of phosphoric acid and other metal ions. Effective treatment and utilization of raffinate acid is an important way to reduce environmental pollution, recycle resources and achieve sustainable development. At present, raffinate acid has been used to prepare agricultural fertilizers such as monoammonium phosphate (MAP) and diammonium phosphate (DAP), but there is no report on the preparation of flame-retardant APP. Summary of the invention
[0004] The invention provides a method for preparing flame-retardant ammonium polyphosphate by using raffinate acid.
[0005] The scheme of the present invention is:
[0006] A method for preparing flame-retardant ammonium polyphosphate from raffinate acid comprises the following steps:
[0007] 1) First, add the raffinate into the neutralization reactor, start stirring, and introduce ammonia gas for neutralization reaction to obtain MAP slurry;
[0008] 2) introducing MAP slurry into a polymerization reactor, and adding urea and phosphorus pentoxide; the polymerization reactor is stirred at a frequency of 20 to 40 Hz; and the reaction time is 4 to 6 hours;
[0009] 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to finally obtain a flame-retardant ammonium polyphosphate product.
[0010] As a preferred technical solution, the 1) neutralization reaction of the raffinate acid P 2 O 5 Content ≥40wt%.
[0011] As a preferred technical solution, the neutralization reaction pressure of 1) is normal pressure, the reaction time is 2 to 4 hours, the stirring frequency is 15 to 25 Hz, the neutralization degree of the product MAP slurry is 0.5 to 0.8, and the P in the MAP slurry is 2 O 5 The content is 40-46wt%, and the N content is 2-6wt%.
[0012] As a preferred technical solution, the mass ratio of the raw materials for the polymerization reaction 2) is MAP slurry: urea: phosphorus pentoxide = 1: 0.5 to 1: 0 to 0.5. The polymerization reaction temperature 2) is 190 to 250°C.
[0013] As a preferred technical solution, the polymerization reaction pressure of 2) is normal pressure; in 2), MAP and urea are first added to the polymerization reactor, and the reaction materials successively go through four states: melting (120°C-130°C, urea melts into MAP slurry), foaming (130°C-160°C, polymerization reaction begins, gas is released), solidification (160°C-170°C, material begins to be viscous), and pulverization (170°C-190°C, material becomes powdery); MAP slurry contains water, and after most of the water evaporates, the material begins to solidify, and then the reactant phosphorus pentoxide is added to the reaction system to continue the reaction; after pulverization, ammonia gas is introduced into the reaction system at a rate of 5-10L / min. Providing an ammonia environment to prevent ammonium polyphosphate from being decomposed by heat and increase the degree of polymerization of the product.
[0014] As a preferred technical solution, when the polymerization reaction 2) is about to be completed, 20 to 30 minutes before the completion of the reaction, melamine is added as a capping agent, and the melamine accounts for 3‰ to 6‰ of the total mass of the MAP slurry, urea and phosphorus pentoxide.
[0015] As a preferred technical solution, after the reaction in step 3) is completed, the material is cooled to a temperature of 30-40° C. and the sieved particle size is less than 4 mm.
[0016] As a preferred technical solution, the packaged flame retardant ammonium polyphosphate product P 2 O 5 Content ≥40wt%, N content ≥10wt%, solubility ≤4.0%.
[0017] The invention also discloses an application of flame-retardant ammonium polyphosphate prepared by a method for preparing flame-retardant ammonium polyphosphate using raffinate acid. The prepared flame-retardant ammonium polyphosphate product uses an addition amount of 13wt% to increase the limiting oxygen index (LOI) of polyurethane rigid foam from 19.5% to 24.3%.
[0018] As a preferred technical solution, a method for preparing a flame retardant comprises the following steps: 40 parts by weight of ammonium polyphosphate, 100 parts by weight of white material, and 168 parts by weight of black material are foamed to obtain a flame retardant polyurethane rigid foam, wherein the flame retardant content is 13%, and the LOI is increased from 19.5% of the pure polyurethane rigid foam to 25.3%. The white material is a composite polyether, and the black material is an isocyanate.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The method of the present invention has a high yield of the product, a simple and easy-to-control reaction process, simple process operation, and high safety; the reaction process is relatively stable and the reaction time is short, the energy consumption is low, and it is environmentally friendly; in addition, the use of the byproduct of wet-process phosphoric acid, the raffinate acid, as a raw material to produce flame-retardant ammonium polyphosphate has a huge cost advantage, which significantly reduces the production cost.
[0021] (2) The present invention develops a process for preparing flame-retardant ammonium polyphosphate using raffinate acid, provides a way to recycle raffinate acid, and promotes the efficient utilization of phosphorus resources.
[0022] (3) The synthesis process of the present invention is simple, the reaction control is simple, and the operation process is safe; the process is stable and controllable, the reaction time is short, the yield is high, the energy consumption is low, the environmental pollution is small, and no additional solvent is required during the reaction process. DETAILED DESCRIPTION
[0023] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0024] Embodiment 1:
[0025] 1) The raffinate (P 2 O 5 :40.87%、FeO 3 :2.06%、Al 2 O 3 :2.66%, MgO: 2.88%, SO 4 2-:6.12%, F:1.06%, SS:7.84%) were pumped into the reactor through an acid pump, and ammonia was passed at 5L / min for neutralization reaction. The stirring rate was 20Hz, the reaction time was 3h, the reaction pressure was normal pressure, and the neutralization degree of MAP slurry was controlled to be 0.5. After the reaction, MAP slurry was obtained. 2 O 5 The content is 40wt%, and the N content is 2wt%.
[0026] 2) According to the mass ratio, MAP slurry: urea: P 2 O 5 =1:0.7:0.1 Obtain the reaction raw materials, first add MAP slurry and urea into the polymerization reactor, the reaction temperature is gradually increased from 120°C to 190°C, the stirring rate is 40Hz, the reaction materials successively go through melting (120°C-130°C, urea melts into MAP slurry, reaction time 40min), foaming (130°C-160°C, polymerization reaction begins, gas is released, reaction time 40min), solidification (160°C-170°C, material begins to be viscous, reaction time 20min), pulverization (170°C-190°C, material becomes powder state) 4 states, after the material begins to solidify, add reactant P to the reaction system 2 O 5 , continue the reaction, after the powder is pulverized, introduce ammonia into the reaction system at a rate of 5L / min; the total reaction time is 5h. 30min before the completion of the reaction, add melamine as a capping agent (5‰ of the total mass) and wait for the reaction to complete.
[0027] 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to obtain qualified products.
[0028] Embodiment 2:
[0029] 1) The raffinate acid was pumped into the reactor through an acid pump, and ammonia was passed at 8 L / min for neutralization reaction. The stirring rate was 20 Hz, the reaction time was 3 h, the reaction pressure was normal pressure, and the neutralization degree of MAP slurry was controlled to be 0.8. After the reaction, MAP slurry was obtained. 2 O 5 The content is 43wt%, and the N content is 3wt%.
[0030] 2) According to the mass ratio, MAP slurry: urea: P 2 O 5=1:0.7:0.1 Obtain the reaction raw materials, first add MAP slurry and urea into the polymerization reactor, the reaction temperature is gradually increased from 120°C to 220°C, the stirring rate is 40Hz, the reaction materials successively go through melting (120°C-130°C, urea melts into MAP slurry, reaction time 40min), foaming (130°C-160°C, polymerization reaction begins, gas is released, reaction time 40min), solidification (160°C-170°C, the material begins to be viscous, reaction time 20min), pulverization (170°C-220°C, the material becomes powdered state) 4 states, after the material begins to solidify, add reactant P to the reaction system 2 O 5 , continue the reaction, after powderization, introduce ammonia into the reaction system at a rate of 5L / min; the reaction time is 5h, 30min before the completion of the reaction, add melamine as a capping agent (5‰ of the total mass), and wait for the reaction to be completed.
[0031] 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to obtain qualified products.
[0032] Embodiment 3:
[0033] 1) The raffinate acid was pumped into the reactor through an acid pump, and ammonia was passed at 10 L / min for neutralization reaction. The stirring rate was 20 Hz, the reaction time was 3 h, the reaction pressure was normal pressure, and the neutralization degree of MAP slurry was controlled to be 0.6. After the reaction, MAP slurry was obtained. 2 O 5 The content is 46wt%, and the N content is 6wt%.
[0034] 2) According to the mass ratio, MAP slurry: urea: P 2 O 5 =1:0.7:0.1 Obtain the reaction raw materials, first add MAP slurry and urea into the polymerization reactor, the reaction temperature is gradually increased from 120°C to 250°C, the stirring rate is 40Hz, the reaction materials successively go through melting (120°C-130°C, urea melts into MAP slurry, reaction time 40min), foaming (130°C-160°C, polymerization reaction begins, gas is released, reaction time 40min), solidification (160°C-170°C, material begins to be viscous, reaction time 20min), pulverization (170°C-250°C, material becomes powder state) 4 states, after the material begins to solidify, add reactant P to the reaction system 2 O 5 , continue the reaction, after powderization, introduce ammonia into the reaction system at a rate of 5L / min; the reaction time is 5h, 30min before the completion of the reaction, add melamine as a capping agent (5‰ of the total mass), and wait for the reaction to be completed.
[0035] 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to obtain qualified products.
[0036] Embodiment 4:
[0037] 1) The raffinate acid was pumped into the reactor through an acid pump, and ammonia was passed at 10 L / min for neutralization reaction. The stirring rate was 20 Hz, the reaction time was 3 h, the reaction pressure was normal pressure, and the neutralization degree of MAP slurry was controlled to be 0.6. After the reaction, MAP slurry was obtained. 2 O 5 The content is 46wt%, and the N content is 6wt%.
[0038] 2) According to the mass ratio, MAP slurry: urea: P 2 O 5 =1:0.56:0 to obtain the reaction raw materials, first add MAP slurry and urea into the polymerization reactor, the reaction temperature is gradually increased from 120°C to 250°C, the stirring rate is 40Hz, the reaction materials successively go through melting (120°C-130°C, urea melts into MAP slurry, reaction time 40min), foaming (130°C-160°C, polymerization reaction begins, gas is released, reaction time 40min), curing (160°C-170°C, the material begins to be viscous, reaction time 20min), pulverization (170°C-250°C, the material becomes powder state) 4 states, after pulverization, ammonia is introduced into the reaction system at a rate of 5L / min; the reaction time is 5h, 30min before the completion of the reaction, melamine is added as a capping agent (5‰ of the total mass), and the reaction is waited for completion.
[0039] 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to obtain qualified products.
[0040] The products of Examples 1 to 4 were tested, and the results were as shown in Table 1:
[0041] Table 1 Testing indicators of flame retardant ammonium polyphosphate products
[0042] index Example 1 Example 2 Example 3 Example 4 Total nitrogen (N) / % 17.2 16.2 14.8 14.9 <![CDATA[Phosphorus content (P 2 O 5 ) / %]]> 46.9 48.1 49.4 49.1 PH 7.51 7.35 7.33 7.32 <![CDATA[Water solubility g / 100mL H 2 O]]> 3.87 3.37 2.23 2.86
[0043] According to the present invention, the synthesis process of the product index embodiment 3 in the above embodiment is the best, that is, the mass ratio of the reaction is MAP slurry: urea: P 2 O 5=1:0.7:0.1, reaction temperature is 250℃, reaction pressure is normal pressure, stirring rate is 40Hz, reaction time is 5h. This product is used in flame retardant polyurethane rigid foam. 40 parts of ammonium polyphosphate, 100 parts of white material (combined polyether), and 168 parts of black material (isocyanate) are foamed to obtain flame retardant polyurethane rigid foam. The addition of 13wt% can increase the LOI of polyurethane rigid foam from 19.5% to 25.3%.
[0044] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing flame-retardant ammonium polyphosphate from raffinate acid, It is characterized in that The following steps are involved: 1) First, add the raffinate into the neutralization reactor, start stirring, and introduce ammonia gas for neutralization reaction to obtain MAP slurry; 2) introducing MAP slurry into a polymerization reactor, and adding urea and phosphorus pentoxide; the stirring frequency of the polymerization reactor is 20 to 40 Hz; and the reaction time is 4 to 6 hours; 3) After the reaction is completed, the material is cooled, crushed, screened and packaged to finally obtain a flame-retardant ammonium polyphosphate product.
2. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: 1) P in the raffinate used in the neutralization reaction 2 O 5 Content ≥40wt%.
3. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: The neutralization reaction pressure of 1) is normal pressure, the reaction time is 2 to 4 hours, the stirring frequency is 15 to 25 Hz, and the neutralization degree of the product MAP slurry is 0.5 to 0.
8.
4. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: The mass ratio of the raw materials for the polymerization reaction 2) is MAP slurry: urea: phosphorus pentoxide = 1: 0.5 to 1: 0 to 0.5, and the polymerization reaction temperature is 190° C. to 250° C.
5. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: The polymerization reaction pressure of 2) is normal pressure; in 2), MAP and urea are first added to the polymerization reactor, and the reaction materials successively go through four states: melting, foaming, solidification, and pulverization; after the materials begin to solidify, phosphorus pentoxide is added to the reaction system to continue the reaction; after pulverization, ammonia is introduced into the reaction system at a rate of 5 to 10 L / min.
6. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: 2) When the polymerization reaction is about to be completed, melamine is added as a capping agent, and the melamine accounts for 3‰ to 6‰ of the total mass of the MAP slurry, urea and phosphorus pentoxide.
7. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: After the reaction in step 3) is completed, the material is cooled to a temperature of 30-40° C. and the sieved particle size is less than 4 mm.
8. A method for preparing flame-retardant ammonium polyphosphate using raffinate as claimed in claim 1, Features: 3) Flame retardant ammonium polyphosphate product P after packaging 2 O 5 Content ≥40wt%, N content ≥10wt%, solubility ≤4.0%.
Citation Information
Patent Citations
Method for preparing industrial grade monoammonium phosphate by using raffinate acid through twice neutralizational process
CN103896232A
Production of ii type ammonium polyphosphate
JP1999302006A
Cited By
Process for the preparation of ammonium polyphosphate from raffinate acid
CN123026201A