Lithium ion battery positive electrode material and preparation method and application thereof
The reaction of metallic iron or manganese with phosphoric acid produces ferrous dihydrogen phosphate or manganese dihydrogen phosphate, which is co-precipitated with lithium-containing solution at low temperature and then sintered. This solves the problem of poor batch stability and high energy consumption in the production of lithium-ion battery cathode materials. To solve the problem, a lithium iron (manganese) phosphate cathode material with stable structure and excellent performance was obtained, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202410750783.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing production process of lithium-ion battery cathode materials has problems such as poor batch stability, high energy consumption, and unfriendly environment. It is difficult to obtain lithium iron (manganese) phosphate materials with stable structure and excellent performance.
The reaction of metallic iron or manganese with phosphoric acid to produce ferrous dihydrogen phosphate or manganese dihydrogen phosphate is used as the reaction raw material. Through low-temperature thermal reaction and lithium-containing solution co-precipitation under the synergistic effect of pH regulator, subsequent sintering is used to prepare iron (manganese) phosphate. Lithium cathode material.
The lithium iron (manganese) phosphate cathode material with stable structure and excellent performance can be obtained in the next step at low temperature, which reduces energy consumption and cost and is suitable for industrial applications.
Smart Images

Figure CN118754077A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a lithium ion battery positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium iron (manganese) phosphate (lithium iron phosphate, lithium manganese phosphate, lithium manganese iron phosphate) is a new type of lithium-ion battery electrode material. Its characteristics are large discharge capacity, low price, non-toxicity, and no environmental pollution. Realizing industrial production is the focus of our research.
[0003] The production processes of lithium iron (manganese) phosphate are different. The current mainstream processes are as follows: one is a high-temperature solid phase method using lithium carbonate and iron (manganese) phosphate as raw materials, such as CN105789620A discloses a preparation method of lithium iron phosphate positive electrode material and a lithium iron phosphate positive electrode material. The preparation method of the present application includes preparing lithium iron phosphate by a solid phase synthesis method, which includes ball milling and high-temperature calcination. Acetylene is introduced into an inert atmosphere during calcination to form carbon nanotubes inside and between the generated lithium iron phosphate particles to obtain a highly conductive lithium iron phosphate positive electrode material. ; The second is a sol-gel method using iron (manganese) nitrate as a raw material. For example, CN102903915A discloses a sol-gel method for preparing a positive electrode material, lithium iron phosphate, wherein manganese salt, lithium salt, chelating agent and phosphate in a molar ratio of 1.9-2.1:1.9-2.1:0.95-1.1:1.9-2.1 are dissolved in water and mixed evenly, ammonia water is used to adjust the pH to 8-10, stirred until viscous, dried, sintered at 600°C-700°C in a non-oxidizing atmosphere for 12-24h, and cooled to obtain lithium iron phosphate. ; The third is a high-temperature and high-pressure hydrothermal or solvent thermal method using ferrous (manganese) sulfate as a raw material, such as the hydrothermal synthesis method of lithium manganese phosphate nanoparticles, a positive electrode material for lithium ion batteries, disclosed in CN104183844A, which uses deionized water as a solvent, a manganese source, a lithium source, and phosphoric acid as reaction materials, a block copolymer as a template, and potassium hydroxide as a mineralizer to promote the nucleation and growth of lithium manganese phosphate, and then performs a heat treatment at a high temperature and high pressure, and then performs a sintering treatment at 550-650°C under the protection of a nitrogen or argon atmosphere to obtain lithium manganese phosphate nanoparticles.
[0004] The high-temperature solid-phase method is to grind lithium carbonate and iron (manganese) phosphate at high energy and then calcine them. It is difficult to make the mixture of two different substances very uniform, and the batch stability is poor, which makes the performance of the prepared lithium iron phosphate slightly insufficient. In addition, the grinding takes a long time and consumes a lot of energy. The sol-gel method produces a large amount of nitrogen-containing compounds in the actual production process, which is extremely unfriendly to the environment. The hydrothermal or solvent thermal method has high requirements for equipment and high energy consumption due to high temperature and high pressure, and is rarely used in industry.
[0005] Therefore, how to obtain lithium iron (manganese) phosphate positive electrode materials with stable structure and excellent performance while reducing costs is a technical problem that needs to be solved urgently. Summary of the invention
[0006] In view of the shortcomings of the prior art, the present invention aims to provide a positive electrode material for lithium-ion batteries and a preparation method and application thereof. The preparation method provided by the present invention uses ferrous dihydrogen phosphate or manganese dihydrogen phosphate generated by the reaction of inexpensive metallic iron or manganese with phosphoric acid as a reaction raw material, and the reaction raw material and the lithium-containing solution can react at low temperature, and after subsequent sintering, a lithium iron (manganese) phosphate positive electrode material with stable structure and excellent performance is obtained; and the preparation method is simple to operate, low in cost, and suitable for industrial application.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing a positive electrode material for a lithium ion battery, the preparation method comprising the following steps:
[0009] (1) mixing a single metal with a phosphoric acid solution, reacting the mixture, and obtaining a metal phosphate solution, wherein the single metal comprises single iron and / or single manganese;
[0010] (2) mixing the metal phosphate solution, the lithium-containing solution and the pH adjusting agent solution, and subjecting them to a thermal reaction to obtain a reaction product;
[0011] (3) Mixing the reaction product with a carbon source and sintering to obtain the lithium-ion battery positive electrode material.
[0012] The preparation method provided by the present invention uses ferrous dihydrogen phosphate or manganese dihydrogen phosphate generated by the reaction of metal (elemental iron and / or elemental manganese) and phosphoric acid as a reaction raw material, the reaction raw material provides a metal source and a phosphorus source at the same time, and the reaction raw material and the lithium-containing solution can be co-precipitated at low temperature (thermal reaction) under the synergistic effect of a pH regulator to obtain a lithium iron (manganese) phosphate precipitate in one step, and after subsequent sintering, a lithium iron (manganese) phosphate positive electrode material with a stable structure and excellent performance is obtained; and the preparation method is simple to operate, does not need to be carried out in high-voltage equipment, reduces energy consumption and costs, and is suitable for industrial applications.
[0013] Preferably, the molar concentration of the phosphoric acid solution in step (1) is 2 to 10 mol / L, for example, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L or 10 mol / L, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0014] Preferably, in step (1), the molar ratio of the elemental metal to phosphoric acid is 1:(2-5), for example 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5 or 1:5, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0015] Preferably, the reaction temperature in step (1) is 0-65°C, for example, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C or 65°C, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] Preferably, the reaction time of step (1) is 2 to 8 hours, for example 2 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0017] Preferably, the pH value of the metal phosphate solution in step (1) is 0.5-4, for example, 0.5, 0.8, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.3, 3.5, 3.8 or 4, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] In the present invention, the pH value of the metal phosphate solution after the reaction is regulated to be 0.5-4, thereby providing the required pH environment for the reaction.
[0019] Preferably, in step (2), the ratio of the molar amount of lithium in the lithium-containing solution to the molar amount of metal in the metal phosphate solution is (1-3.1):1, for example 1:1, 1.02:1, 1.17:1, 1.3:1, 1.5:1, 1.8:1, 1.94:1, 2:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.85:1, 2.9:1, 3:1 or 3.1:1, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0020] Preferably, the lithium-containing solution in step (2) is an acidic lithium-containing solution, and the pH value of the acidic lithium-containing solution is 1 to 5, for example, 1, 1.3, 1.5, 1.8, 2, 2.3, 2.5, 2.8, 3, 3.3, 3.5, 3.8, 4, 4.3, 4.5, 4.8 or 5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] In the present invention, when the lithium-containing solution is an acidic solution, it not only serves as a lithium source, but also plays a role in adjusting the pH value required for the generation of the target product;
[0022] It should be noted that the preparation process of the lithium-containing solution provided by the present invention is a conventional technical means, and the raw materials and methods of the lithium-containing solution can be obtained, and the present invention is applicable; illustratively, the present invention provides a preparation process of a lithium-containing solution:
[0023] Weigh lithium salt, add deionized water to dissolve it in a solid-liquid ratio of 1: (4-20), add acid to adjust the pH value, and prepare a lithium-containing solution as a lithium source for standby use;
[0024] Optionally, the lithium salt includes but is not limited to at least one of lithium hydroxide, lithium sulfate, lithium chloride, lithium dihydrogen phosphate, lithium acetate, lithium phosphate, dilithium hydrogen phosphate or lithium nitrate; the acid includes but is not limited to at least one of sulfuric acid, phosphoric acid, hydrochloric acid, ascorbic acid, citric acid or acetic acid.
[0025] Preferably, in step (2), the ratio of the molar amount of the pH adjuster to the molar amount of the metal in the metal phosphate solution is (0-2.5):1, for example 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.43:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.97:1, 1:1, 1.17:1, 1.2:1, 1.3:1, 1.5:1, 1.8:1, 2:1, 2.2:1, 2.3:1, 2.4:1, 2.42:1 or 2.5:1, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] In the present invention, by adjusting the dosage of the metal phosphate solution, the lithium-containing solution and the pH regulator solution, it is ensured that the metal (iron and / or manganese), phosphorus and lithium are precipitated together in a suitable ratio, so that the corresponding iron phosphate (manganese) precipitation product is obtained through thermal reaction.
[0027] Preferably, the pH adjuster in step (2) comprises an alkaline pH adjuster.
[0028] Preferably, the pH adjusting agent in step (2) comprises any one of lithium hydroxide, dilithium hydrogen phosphate, sodium hydroxide, potassium hydroxide or ammonia water, or a combination of at least two thereof; typical but non-limiting combinations include a combination of lithium hydroxide and dilithium hydrogen phosphate, a combination of dilithium hydrogen phosphate and sodium hydroxide, a combination of potassium hydroxide and ammonia water, a combination of lithium hydroxide and ammonia water, and the like.
[0029] Preferably, the mixing in step (2) is carried out under a protective atmosphere.
[0030] In the present invention, the protective atmosphere includes a nitrogen atmosphere or an inert gas atmosphere (inert gas such as argon, helium, etc.).
[0031] Preferably, the mixing temperature in step (2) is 80-95°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C or 95°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the mixing method in step (2) comprises:
[0033] With the lithium-containing solution as the base solution, the metal phosphate solution and the pH regulator solution are added into the lithium-containing solution in parallel.
[0034] Preferably, the time for the parallel addition is 1 to 8 hours, for example 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, the thermal reaction in step (2) is carried out under a protective atmosphere.
[0036] Preferably, the temperature of the thermal reaction in step (2) is 80-95°C, for example, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C or 95°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] In the present invention, the temperature of the thermal reaction in step (2) does not need to be too high to obtain the precipitation reactant of lithium iron (manganese) phosphate, and no high-pressure environment is required, and the reaction can be completed directly under standard atmospheric pressure and a protective atmosphere.
[0038] Preferably, the thermal reaction time in step (2) is 2 to 8 hours, for example 3 hours, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] Preferably, the sintering temperature in step (3) is 550-850°C, for example, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C or 850°C, and the sintering time is 4-24h, for example, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h, etc.
[0040] As a preferred technical solution, the preparation method comprises the following steps:
[0041] (1) mixing a single metal with a phosphoric acid solution having a molar concentration of 2 to 10 mol / L, wherein the molar ratio of the single metal to the phosphoric acid is 1:(2 to 5), reacting at 0 to 65° C. for 2 to 8 hours to obtain a metal phosphate solution having a pH value of 0.5 to 4, wherein the single metal comprises single iron and / or single manganese;
[0042] (2) in a protective atmosphere, mixing a metal phosphate solution, a lithium-containing solution having a pH value of 1 to 5, and an alkaline pH adjusting agent solution, and subjecting the mixture to a thermal reaction at 80 to 95° C. for 2 to 8 hours to obtain a reaction product;
[0043] (3) mixing the reaction product with a carbon source and sintering to obtain the positive electrode material for a lithium-ion battery;
[0044] Wherein, in step (2), the ratio of the molar amount of lithium in the lithium-containing solution to the molar amount of metal in the metal phosphate solution is (1-3.1):1; and the ratio of the molar amount of the pH regulator to the molar amount of the metal in the metal phosphate solution is (0-2.5):1.
[0045] In a second aspect, the present invention provides a lithium-ion battery positive electrode material, which is prepared by the preparation method described in the first aspect, and the lithium-ion battery positive electrode material includes any one of lithium iron phosphate, lithium manganese phosphate or lithium manganese iron phosphate, or a combination of at least two of them.
[0046] In a third aspect, the present invention further provides a lithium ion battery, wherein the lithium ion battery comprises the lithium ion battery positive electrode material as described in the second aspect.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The preparation method provided by the present invention uses ferrous dihydrogen phosphate or manganese dihydrogen phosphate generated by the reaction of metal (elemental iron and / or elemental manganese) and phosphoric acid as a reaction raw material, the reaction raw material provides a metal source and a phosphorus source at the same time, and the reaction raw material and the lithium-containing solution can be co-precipitated at low temperature (thermal reaction) under the synergistic effect of a pH regulator, so that a lithium iron (manganese) phosphate precipitate is obtained in one step, and after subsequent sintering, a lithium iron (manganese) phosphate positive electrode material with a stable structure and excellent performance is obtained; and the preparation method is simple to operate, does not need to be carried out in high-voltage equipment, reduces energy consumption and cost, has a short production cycle, and is suitable for industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 This is the XRD pattern of lithium iron phosphate obtained by the preparation method provided in Example 1.
[0050] Figure 2 This is the XRD pattern of lithium manganese iron phosphate obtained by the preparation method provided in Example 7. DETAILED DESCRIPTION
[0051] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0052] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0053] Example 1
[0054] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, and the preparation method is as follows:
[0055] (1) 110 g of iron powder (1.96 mol) was added to a 7 mol / L phosphoric acid solution (the molar ratio of iron to phosphoric acid was 1:3), stirring was started and the temperature was controlled to 50° C., reacted for 2 hours and then filtered to obtain a ferrous dihydrogen phosphate solution; 250 ml of deionized water was added to the above solution to obtain a ferrous dihydrogen phosphate solution with a pH value of 0.8;
[0056] Weigh 48.2 g of lithium hydroxide (2.00 mol), add 800 mL of deionized water to dissolve, add phosphoric acid to adjust the pH value to 4.5, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to iron in the ferrous dihydrogen phosphate solution is 1.0.2:1);
[0057] Weigh 200 g of lithium hydroxide monohydrate (4.76 mol), add 300 mL of deionized water to prepare a pH regulator solution for standby use (the molar ratio of lithium in the pH regulator to iron in the ferrous dihydrogen phosphate solution is 2.42:1);
[0058] (2) placing a lithium-containing bottom liquid in a reaction kettle as a bottom liquid, heating it to 90° C. and introducing nitrogen, and simultaneously adding the ferric dihydrogen phosphate solution and the pH regulator solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 2 hours. After the feeding is completed, the reaction mixture is kept warm in a reaction environment of 90° C. for 3 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium iron phosphate precipitation reactant;
[0059] (3) The lithium iron phosphate precipitation reaction product obtained above was coated with liquid phase glucose (the carbon content of the final lithium iron phosphate positive electrode material was 1.5%), and then sintered at 720° C. for 2 h in a nitrogen atmosphere to obtain the lithium iron phosphate positive electrode material.
[0060] Figure 1 The XRD pattern of lithium iron phosphate obtained by the preparation method provided in Example 1 is shown. Figure 1 It can be seen that the lithium iron phosphate prepared in this example has a high degree of coincidence with the standard card, indicating that the structure is stable and no obvious impurities appear.
[0061] Example 2
[0062] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, and the preparation method is as follows:
[0063] (1) taking 100 g of iron powder (1.80 mol) and adding it to a 3 mol / L phosphoric acid solution (the molar ratio of iron to phosphoric acid is 1:2), stirring and controlling the temperature to 10° C., reacting for 2 hours and then filtering to obtain a ferrous dihydrogen phosphate solution; adding 400 ml of deionized water to the above solution to obtain a ferrous dihydrogen phosphate solution with a pH value of 1;
[0064] Weigh 363 g of lithium sulfate (3.3 mol), add 1000 mL of deionized water to dissolve, add phosphoric acid to adjust the pH value to 4.5, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to iron in the ferrous dihydrogen phosphate solution is 1.83:1);
[0065] Weigh 50.4 g of lithium hydroxide (2.1 mol), add 550 mL of deionized water to prepare a pH regulator solution for standby use (the molar ratio of lithium in the pH regulator to iron in the ferrous dihydrogen phosphate solution is 1.17:1);
[0066] (2) placing a lithium-containing bottom liquid in a reaction kettle as a bottom liquid, heating it to 85° C. and introducing nitrogen, and simultaneously adding the ferric dihydrogen phosphate solution and the pH regulator solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 4 hours. After the feeding is completed, the reaction mixture is kept warm in a reaction environment of 85° C. for 2 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium iron phosphate precipitation reactant;
[0067] (3) The lithium iron phosphate precipitation reaction product obtained above was coated with glucose in liquid phase (the carbon content of the final lithium iron phosphate positive electrode material was 1.5%), and then sintered at 750° C. for 2 h in a nitrogen atmosphere to obtain the lithium iron phosphate positive electrode material.
[0068] Example 3
[0069] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, and the preparation method is as follows:
[0070] (1) taking 100 g of iron (1.80 mol), adding it to a 3.5 mol / L phosphoric acid solution (the molar ratio of iron to phosphoric acid is 1:5), starting stirring and controlling the temperature to 25° C., reacting for 2 hours, and then filtering to obtain a ferrous dihydrogen phosphate solution; adding 300 mL of deionized water to the above solution to obtain a ferrous dihydrogen phosphate solution with a pH value of 2.5;
[0071] Weigh 364 g of lithium dihydrogen phosphate (3.5 mol), add 1000 mL of deionized water to dissolve, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to iron in the ferrous dihydrogen phosphate solution is 1.94:1);
[0072] Weigh 79.8 g of lithium dihydrogen phosphate (0.78 mol), add 450 mL of deionized water to prepare a pH regulator solution for later use (the molar ratio of lithium in the pH regulator to iron in the ferrous dihydrogen phosphate solution is 0.43:1);
[0073] (2) placing a lithium-containing bottom liquid in a reaction kettle as a bottom liquid, heating it to 92° C. and introducing nitrogen, and simultaneously adding the ferric dihydrogen phosphate solution and the pH regulator solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 2.5 hours. After the feeding is completed, the reaction mixture is kept warm in a reaction environment of 92° C. for 2 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium iron phosphate precipitation reactant;
[0074] (3) The lithium iron phosphate precipitation reaction product obtained above was coated with glucose in liquid phase (the carbon content of the final lithium iron phosphate positive electrode material was 1.3%), and then sintered at 760° C. for 3 h in a nitrogen atmosphere to obtain the lithium iron phosphate positive electrode material.
[0075] Example 4
[0076] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, and the preparation method is as follows:
[0077] (1) taking 100 g of iron powder (1.80 mol), adding it to a 4.5 mol / L phosphoric acid solution (the molar ratio of iron to phosphoric acid is 1:3), starting stirring and controlling the temperature to 45° C., reacting for 2 hours, and then filtering to obtain a ferrous dihydrogen phosphate solution; adding 200 mL of deionized water to the above solution to obtain a ferrous dihydrogen phosphate solution with a pH value of 1.5;
[0078] Weigh 216 g of lithium chloride (5.14 mol), add 1000 mL of deionized water to dissolve, add phosphoric acid to adjust the pH value to 4.5, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to iron in the ferrous dihydrogen phosphate solution is 2.85:1);
[0079] Weigh 65 g of sodium hydroxide (1.625 mol), add 350 mL of deionized water to prepare a pH regulator solution for later use (the molar ratio of lithium in the pH regulator to iron in the ferrous dihydrogen phosphate solution is 0:1);
[0080] (2) placing a lithium-containing bottom liquid in a reaction kettle as a bottom liquid, heating it to 88° C. and introducing nitrogen, and simultaneously adding the ferric dihydrogen phosphate solution and the pH regulator solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 2 hours. After the feeding is completed, the reaction mixture is kept warm in a reaction environment of 88° C. for 6 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium iron phosphate precipitation reactant;
[0081] (3) The lithium iron phosphate precipitation reaction product obtained above was coated with liquid phase glucose (the carbon content of the final lithium iron phosphate positive electrode material was 1.35%), and then sintered at 700° C. for 3 h in a nitrogen atmosphere to obtain the lithium iron phosphate positive electrode material.
[0082] Example 5
[0083] This embodiment provides a method for preparing a lithium manganese phosphate positive electrode material, and the preparation method is as follows:
[0084] (1) taking 100 g of manganese powder (1.8 mol), adding it to a 6 mol / L phosphoric acid solution (the molar ratio of manganese to phosphoric acid is 1:3), starting stirring and controlling the temperature to 65° C., reacting for 2 hours, and then filtering to obtain a dihydrogen manganese phosphate solution; adding 250 ml of deionized water to the above solution to obtain a dihydrogen manganese phosphate solution with a pH value of 1.5;
[0085] Weigh 458 g of lithium dihydrogen phosphate (4.4 mol), add 1200 mL of deionized water to dissolve, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to manganese in the manganese dihydrogen phosphate solution is 2.4:1);
[0086] Weigh 42 g of lithium hydroxide (1.75 mol), add 500 mL of deionized water to prepare a pH regulator solution for later use (the molar ratio of lithium in the pH regulator to manganese in the dihydrogen manganese phosphate solution is 0.97:1);
[0087] (2) placing a lithium-containing bottom liquid in a reaction kettle as a bottom liquid, heating it to 95° C. and introducing nitrogen, and simultaneously adding the manganese dihydrogen phosphate solution and the pH adjusting agent solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 1 hour. After the feeding is completed, the reaction mixture is kept warm in a reaction environment of 95° C. for 4 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium manganese phosphate precipitation reaction product;
[0088] (3) The lithium manganese phosphate precipitation reaction product obtained above was coated with glucose in liquid phase (the carbon content of the final lithium iron phosphate positive electrode material was 2.5%), and then sintered at 700° C. for 8 h in a nitrogen atmosphere to obtain the lithium manganese phosphate positive electrode material.
[0089] Example 6
[0090] This embodiment provides a method for preparing a lithium manganese phosphate positive electrode material, and the preparation method is as follows:
[0091] (1) taking 100 g of manganese powder (1.8 mol), adding it to a 5 mol / L phosphoric acid solution, starting stirring and controlling the temperature to 55° C., reacting for 2 hours, and then filtering to obtain a manganese dihydrogen phosphate solution; adding 300 ml of deionized water to the above solution to obtain a manganese dihydrogen phosphate solution with a pH value of 1;
[0092] Weigh 320 g of lithium nitrate (4.64 mol), add 1500 mL of deionized water to dissolve, add nitric acid to adjust the pH value to 4.5, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to manganese in the dihydrogen manganese phosphate solution is 2.6:1);
[0093] Weigh 65 g of potassium hydroxide and add 350 mL of deionized water to prepare a pH regulator solution for later use (the molar ratio of lithium in the pH regulator to manganese in the dihydrogen manganese phosphate solution is 0:1);
[0094] (2) placing the lithium-containing bottom liquid in a reaction kettle as the bottom liquid, heating it to 88° C. and introducing nitrogen, and simultaneously adding the manganese dihydrogen phosphate solution and the pH adjusting agent solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 3 hours. After the feeding is completed, the reaction is kept warm in a reaction environment of 88° C. for 6 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium manganese phosphate precipitation reaction product;
[0095] (3) The lithium manganese phosphate precipitation reaction product obtained above was coated with glucose in liquid phase (the carbon content of the final lithium iron phosphate positive electrode material was 3.0%), and then sintered at 650° C. for 4 h in a nitrogen atmosphere to obtain the lithium manganese phosphate positive electrode material.
[0096] Example 7
[0097] This embodiment provides a method for preparing a lithium manganese iron phosphate positive electrode material, and the preparation method is as follows:
[0098] (1) 88 g of manganese powder (1.6 mol) was added to a 5 mol / L phosphoric acid solution, stirred and the temperature was controlled at 45° C., reacted for 2 hours, and then filtered to obtain a manganese dihydrogen phosphate solution; 12 g of iron powder was weighed and added to a 3 mol / L phosphoric acid solution, stirred and the temperature was controlled at 65° C., reacted for 2 hours, and then filtered to obtain a ferrous dihydrogen phosphate solution; 300 ml of deionized water was added to the mixed solution of the above two solutions to obtain a mixed solution with a pH value of 1.3;
[0099] Weigh 447 g of lithium dihydrogen phosphate (4.3 mol), add 1800 mL of deionized water to dissolve, and prepare a lithium-containing solution (base solution) for standby use (the molar ratio of lithium in the lithium-containing solution to manganese in the manganese dihydrogen phosphate solution is 2.7:1);
[0100] Weigh 46.2 g of lithium hydroxide (1.925 mol), add 350 mL of deionized water to prepare a pH regulator solution for later use (the molar ratio of lithium in the pH regulator to manganese in the dihydrogen manganese phosphate solution is 1.2:1);
[0101] (2) placing the lithium-containing bottom liquid in a reaction kettle as the bottom liquid, heating it to 88° C. and introducing nitrogen, and simultaneously adding the manganese dihydrogen phosphate solution and the pH adjusting agent solution prepared in step (1) to the lithium-containing solution (bottom liquid), with a feeding time of 3 hours. After the feeding is completed, the reaction is kept warm in a reaction environment of 88° C. for 5 hours (thermal reaction), and then solid-liquid separation, washing and drying are performed to obtain a lithium iron manganese phosphate precipitation reaction product;
[0102] (3) The lithium manganese iron phosphate precipitation reaction product obtained above was coated with glucose in liquid phase (the carbon content of the final lithium iron phosphate positive electrode material was 1.5%), and then sintered at 750° C. for 3 h in a nitrogen atmosphere to obtain the lithium manganese iron phosphate positive electrode material.
[0103] Figure 2 The XRD pattern of lithium manganese iron phosphate obtained by the preparation method provided in Example 7 is shown. Figure 2 It can be seen that the lithium iron phosphate prepared in this example has a high degree of coincidence with the standard card, indicating that the structure is stable and no obvious impurities appear.
[0104] Comparative Example 1
[0105] The difference between this comparative example and Example 1 is that this comparative example provides a method for preparing lithium iron phosphate by a high-temperature solid phase method:
[0106] Weigh 25 g of battery-grade lithium carbonate, 100 g of battery-grade anhydrous iron phosphate and 10 g of glucose, disperse them in deionized water, and then transfer them to a sand mill for grinding for 0.5 h. The slurry is spray-dried and then sintered at 750 ° C in a tubular furnace under an inert atmosphere for 8 h. After cooling naturally, lithium iron phosphate, a positive electrode material for lithium-ion batteries, is obtained.
[0107] Comparative Example 2
[0108] The difference between this comparative example and Example 5 is that this comparative example provides a method for preparing lithium manganese phosphate by a high-temperature solid phase method:
[0109] Weigh 24.5 g of battery-grade lithium carbonate, 73.8 g of battery-grade anhydrous iron phosphate, 70.6 g of 85% concentrated phosphoric acid and 10 g of glucose, disperse them in deionized water, and then transfer them to a sand mill for grinding for 4 hours. The slurry is spray-dried and then sintered at 730° C. in a tubular furnace under an inert atmosphere for 10 hours and naturally cooled to obtain lithium iron phosphate, a positive electrode material for lithium-ion batteries.
[0110] [Preparation and testing of lithium-ion batteries]
[0111] (a) Pole preparation:
[0112] According to the mass ratio of active material (positive electrode materials provided in Examples 1-7 and Comparative Examples 1-2, respectively): conductive agent (super-p) and polyvinylidene fluoride (PVDF) = 8:1:1, the three materials were weighed and placed in an agate mortar for dry grinding for 15 minutes to mix the three materials evenly, and then transferred to a glass bottle, an appropriate amount of N-methylpyrrolidone (NMP) was added dropwise to adjust the viscosity of the slurry, and after sealing, it was continuously stirred at a speed of 600 rpm for 6 hours to form a uniform slurry, and then it was coated on the rough side of the previously cleaned and dried copper foil by a scraper method, with a coating thickness of about 200 μm, and then transferred to a 110°C oven for pre-drying for 2 hours, and then placed in a 100°C vacuum drying oven for drying for 12 hours; after natural cooling, it was punched into discs with a diameter of 12 mm with a slicer, weighed, sealed and placed in a drying dish for standby use.
[0113] (b) Battery assembly:
[0114] CR2032 button cells were assembled in a glove box filled with high-purity argon atmosphere, where the contents of H2O and O2 were both less than 0.1 ppm. The electrolyte was 1M LiPF6 (EC:EMC:DMC=1:1:1 vol%), and the separator was a PP separator.
[0115] (c) Battery performance test:
[0116] The electrochemical performance of CR2032 button cells was tested using a BlueDian battery test system. The charge and discharge cutoff voltage range was 2.0-4.5 V. The test rates were 0.1C / 0.1C and 1C / 1C, respectively. The test results are shown in Table 1.
[0117] Table 1
[0118]
[0119] From Table 1, we can get:
[0120] From the data results of Examples 1-7, it can be seen that in the present invention, a single metal (iron and / or manganese) is used as a preparation raw material, and the reaction product of lithium iron (manganese) phosphate can be achieved in one step through a thermal reaction at a low temperature; after subsequent sintering, a lithium iron (manganese) phosphate positive electrode material with a stable structure and excellent performance is obtained; and the preparation method is simple to operate, does not need to be carried out in high-voltage equipment, reduces energy consumption and costs, has a short production cycle, and is suitable for industrial applications.
[0121] From the data results of Example 1 and Comparative Example 1, and Example 5 and Comparative Example 2, it can be seen that the preparation method provided by the present invention obtains lithium iron (manganese) phosphate, which has a stable structure, stable batches, excellent performance, and low energy consumption. However, the traditional solid phase method uses a sand mill to grind the raw materials and then sinter at high temperature for a long time to obtain the target product, which has low electrochemical performance and increased energy consumption, which is not conducive to cost reduction in large-scale applications.
[0122] In summary, the preparation method provided by the present invention uses ferrous dihydrogen phosphate or manganese dihydrogen phosphate generated by the reaction of metal (elemental iron and / or elemental manganese) and phosphoric acid as the reaction raw material, and the reaction raw material provides a metal source and a phosphorus source at the same time. The reaction raw material and the lithium-containing solution can be co-precipitated at low temperature (thermal reaction) under the synergistic effect of a pH regulator, and a lithium iron (manganese) phosphate precipitate is obtained in one step. After subsequent sintering, a lithium iron (manganese) phosphate positive electrode material with a stable structure and excellent performance is obtained; and the preparation method is simple to operate, does not need to be carried out in high-voltage equipment, reduces energy consumption and cost, has a short production cycle, and is suitable for industrial applications.
[0123] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a positive electrode material for a lithium ion battery, characterized in that: The preparation method comprises the following steps: (1) mixing a single metal with a phosphoric acid solution, reacting the mixture, and obtaining a metal phosphate solution, wherein the single metal comprises single iron and / or single manganese; (2) mixing the metal phosphate solution, the lithium-containing solution and the pH adjusting agent solution, and subjecting them to a thermal reaction to obtain a reaction product; (3) Mixing the reaction product with a carbon source and sintering to obtain the lithium-ion battery positive electrode material.
2. The preparation method according to claim 1, characterized in that: The molar concentration of the phosphoric acid solution in step (1) is 2 to 10 mol / L; Preferably, in step (1), the molar ratio of the elemental metal to phosphoric acid is 1:(2-5).
3. The preparation method according to claim 1 or 2, characterized in that: The reaction temperature of step (1) is 0 to 65° C.; the reaction time of step (1) is 2 to 8 hours; Preferably, the pH value of the metal phosphate solution in step (1) is 0.5-4.
4. The preparation method according to any one of claims 1 to 3, characterized in that In step (2), the ratio of the molar amount of lithium in the lithium-containing solution to the molar amount of metal in the metal phosphate solution is (1 to 3.1):1; Preferably, the lithium-containing solution in step (2) is an acidic lithium-containing solution, and the pH value of the acidic lithium-containing solution is 1 to 5; Preferably, in step (2), the ratio of the molar amount of the pH adjuster to the molar amount of the metal in the metal phosphate solution is (0-2.5):1; Preferably, the pH adjuster in step (2) comprises an alkaline pH adjuster; Preferably, the pH adjuster in step (2) comprises any one of lithium hydroxide, dilithium hydrogen phosphate, sodium hydroxide, potassium hydroxide or ammonia water, or a combination of at least two thereof.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The mixing in step (2) is carried out under a protective atmosphere; Preferably, the mixing temperature in step (2) is 80-95°C.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The thermal reaction in step (2) is carried out under a protective atmosphere; Preferably, the temperature of the thermal reaction in step (2) is 80-95°C; Preferably, the thermal reaction time in step (2) is 2 to 8 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The sintering temperature in step (3) is 550-850° C., and the sintering time is 4-24 hours.
8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: (1) mixing a single metal with a phosphoric acid solution having a molar concentration of 2 to 10 mol / L, wherein the molar ratio of the single metal to the phosphoric acid is 1:(2 to 5), reacting at 0 to 65° C. for 2 to 8 hours to obtain a metal phosphate solution having a pH value of 0.5 to 4, wherein the single metal comprises single iron and / or single manganese; (2) in a protective atmosphere, mixing a metal phosphate solution, a lithium-containing solution having a pH value of 1 to 5, and an alkaline pH adjusting agent solution, and subjecting the mixture to a thermal reaction at 80 to 95° C. for 2 to 8 hours to obtain a reaction product; (3) mixing the reaction product with a carbon source and sintering to obtain the positive electrode material for a lithium-ion battery; Wherein, in step (2), the ratio of the molar amount of lithium in the lithium-containing solution to the molar amount of metal in the metal phosphate solution is (1-3.1):1; and the ratio of the molar amount of the pH regulator to the molar amount of the metal in the metal phosphate solution is (0-2.5):
1.
9. A positive electrode material for a lithium ion battery, characterized in that: The lithium-ion battery positive electrode material is prepared by the preparation method according to any one of claims 1 to 8, and the lithium-ion battery positive electrode material includes any one of lithium iron phosphate, lithium manganese phosphate or lithium manganese iron phosphate, or a combination of at least two of them.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium-ion battery positive electrode material as claimed in claim 9.
Citation Information
Patent Citations
Preparation method of lithium iron phosphate or lithium manganese iron positive electrode material of lithium ion battery
CN114899392A
Defective nano lithium iron phosphate as well as preparation method and application thereof
CN115477294A
Lithium iron phosphate liquid phase synthesis method
CN115818610A
Preparation method of lithium iron phosphate / lithium iron manganese phosphate positive electrode material
CN118206096A
Method for using amblygonite to prepare lithium-containing compound
WO2020057043A1
Cited By
Lithium manganese iron phosphate positive electrode material with consistent morphology, preparation method and positive electrode
CN121516840A