Method for preparing anthracite / sucrose-based composite carbon material through two-time carbonization

Through the preparation method of double carbonization of anthracite and sucrose, a high-performance composite carbon material is formed, which solves the cost and property control problems of hard carbon and soft carbon materials in industrial applications, and realizes an electrode material with high sodium storage capacity and excellent rate performance. Preparation, has broad commercial application prospects.

CN118754098APending Publication Date: 2024-10-11SICHUAN UNIV

Patent Information

Application Number
CN202410942946.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing hard carbon and soft carbon materials have problems in industrial applications such as high cost, low carbon yield, and difficult to control properties. Moreover, a single material cannot meet the needs of practical applications, making it difficult to prepare high-performance electrode materials.

Method used

Anthracite and sucrose are used as precursors, and a high-performance composite carbon material is prepared through a two-step carbonization preparation method. First, it is pretreated at low temperature to form a cross-linked structure, and then carbonized at high temperature. Potassium hydroxide and hydrochloric acid are used to remove impurities. .

Benefits of technology

The prepared composite carbon material has high sodium storage capacity, excellent rate performance and cycle stability, low cost, environmentally friendly, suitable layer spacing and abundant defects to provide multiple sodium storage active sites, electronic conductivity and ionic conductivity. High efficiency and suitable for commercial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754098A_ABST
    Figure CN118754098A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing an anthracite / sucrose-based composite carbon material through two-time carbonization, which comprises the following steps: sequentially weighing a coal-based soft carbon precursor and a carbohydrate hard carbon precursor according to different proportions, then carrying out ball milling for 12 hours to uniformly mix the two raw materials, and drying at 80 DEG C for 12 hours; transferring the mixed powder obtained in the step (1) into a tubular furnace, heating to 400 DEG C at a heating rate of 5 DEG C / min in a certain atmosphere, keeping the temperature for 2 hours, and then naturally cooling to room temperature along with the furnace, thereby completing the first pretreatment carbonization step to obtain an intermediate; according to the preparation method, simple low-temperature pretreatment is utilized to enable anthracite and cane sugar to generate a cross-linking effect, then potassium hydroxide and hydrochloric acid are used for removing impurities in the raw materials, and finally carbonization is carried out for a certain time at the temperature of 1200 DEG C to prepare the composite carbon material, the used raw materials are only anthracite and cane sugar, the source is wide, the price is low, and the environment-friendly effect is achieved; and medicines, such as potassium hydroxide, hydrogen chloride and the like, required by impurity removal can also be well supplied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of negative electrode materials for sodium ion batteries, and in particular relates to a method for preparing anthracite / sucrose-based composite carbon material by double carbonization. Background Art

[0002] Carbon materials can be divided into soft carbon and hard carbon according to whether they can be converted into graphite at appropriate temperatures. Soft carbon can usually be converted into artificial graphite when heated at a temperature of >3000°C, and its precursors are petroleum coke, needle coke, coal, etc., while hard carbon is a carbon material that cannot be graphitized even when carbonized at a temperature of >3000°C, and its precursors are usually annealed thermosetting precursors, such as resin-based, polymer-based, biomass-based and carbohydrate-based, which will produce a rigid cross-linked structure during the pyrolysis process, thereby inhibiting the growth of parallel carbon layers and giving hard carbon a turbine structure and a disordered structure. The pyrolysis involves multiple steps such as aromatization, polycondensation, the formation and growth of carbon layers, and the release of small molecules. The process is very complicated and the resulting microstructure is also very uneven. In terms of performance, soft carbon usually shows a tilted charge-discharge curve. Due to its relatively ordered carbon layer arrangement and high crystallinity, fewer internal defects and closed pores, the sodium storage capacity is relatively low (about 100mAh / g), and the initial coulombic efficiency is low, but due to its higher conductivity and capacitance-controlled sodium storage mechanism, soft carbon has better rate performance. In contrast, the structural characteristics of highly disordered structure, large interlayer spacing and abundant defects enable hard carbon to achieve a large reversible specific capacity (varying between 250-480mAh / g), and its charge-discharge curve is also quite different from that of soft carbon, showing a tilted voltage area and a low voltage platform below 0.1V. Lower operating voltage can increase battery energy density, but lower conductivity and longer platform area make the sodium storage kinetics of hard carbon slow and the cycle performance poor. In addition, from the perspective of precursors, hard carbon precursors have the advantages of high natural abundance, environmental friendliness, high mechanical strength, and good thermal stability, but they also have many disadvantages, such as the high price of resin-based and polymer-based precursors and too low carbon yield; although biomass-based precursors can reduce costs to a certain extent, their carbon content is low, the uniformity of the precursors cannot be guaranteed, and the properties of the prepared carbon materials are difficult to control; the shortcomings of these precursors have greatly limited the industrial development of hard carbon. Soft carbon precursors are usually aromatic conjugated organic small molecules, such as asphalt, petroleum coke, etc., which are inexpensive and have more cost advantages than hard carbon in commercial applications. Therefore, a single hard carbon or soft carbon cannot meet the needs of actual applications. At present, many studies have designed and regulated the structure of hard carbon materials through pre-oxidation, composite materials, heteroatom doping, surface engineering and other means. Among these strategies, the composite material can overcome the limitations of using hard carbon or soft carbon alone through the synergistic effect of the two precursors. Specifically, the introduction of soft carbon precursors can enhance the overall conductivity and sodium storage kinetics of the composite material, that is, improve the rate performance and cycle stability. At the same time, the hard carbon precursor can provide more sodium storage active sites and increase the specific capacitance.

[0003] In summary, it is of great significance to find suitable precursors to prepare high-performance electrode materials. The technical problem to be solved by the present invention is to provide a method for preparing composite carbon materials with a wide range of raw material sources, low cost, few types of reagents, and simple process. The prepared composite carbon material can maintain a high capacity and has excellent rate performance and cycle stability. Summary of the invention

[0004] The method for preparing anthracite / sucrose-based composite carbon materials by two carbonizations described in the present invention has the following basic idea: first, anthracite and sucrose are evenly mixed by ball milling in different proportions, and after drying, they are pretreated at a lower temperature in different atmospheres for a period of time, that is, the first carbonization is completed to obtain a composite intermediate. The intermediate is treated with a certain concentration of alkali and acid for a period of time in turn to remove impurities; finally, high-temperature carbonization is performed in an inert atmosphere for a certain period of time to prepare a high-performance composite electrode material. The raw materials used in the present invention are low in cost, widely available, environmentally friendly, and have high commercial value; in addition, the preparation method is relatively simple, and the preparation temperature is lower than that of conventional hard carbon preparation, which can further reduce energy consumption. The composite carbon material prepared by the present invention has a low impurity content and stable performance; it has a suitable interlayer spacing, a high degree of disorder and abundant defects, can provide more sodium storage active sites, and has a high sodium storage capacity; at the same time, the composite carbon material in the present invention has high ionic conductivity and electronic conductivity, and the sodium storage kinetics are accelerated, which greatly improves the rate performance and cycle stability of the material.

[0005] The objective of the present invention is achieved through the following technical solutions:

[0006] A method for preparing anthracite / sucrose-based composite carbon material by double carbonization, the steps of which are as follows:

[0007] (1) weighing a coal-based soft carbon precursor and a carbohydrate hard carbon precursor in different proportions, then ball milling the two raw materials for 12 hours to mix them evenly, and drying them at 80° C. for 12 hours;

[0008] (2) transferring the mixed powder obtained in step (1) to a tube furnace, heating it to 400° C. at a heating rate of 5° C. / min under a certain atmosphere, and keeping it at that temperature for 2 hours, and then cooling it naturally to room temperature in the furnace, thus completing the first pretreatment carbonization step and obtaining an intermediate;

[0009] (3) washing the intermediate obtained in step (2) with 5M potassium hydroxide and 5% hydrochloric acid solution to remove impurities, washing with deionized water until neutral, and drying in an oven at 120° C. for 12 hours;

[0010] (4) The intermediate after impurity removal and drying in step (3) is transferred to a tubular furnace, and under the protection of inert gas argon, the temperature is increased to 1200° C. at a heating rate of 5° C. / min and kept at this temperature for 2 hours, and then cooled to room temperature with the furnace, thereby preparing a composite carbon material.

[0011] (5) The carbon material, conductive carbon (Super P li) and binder (PVDF) were mixed in a mass ratio of 90:5:5 and dissolved in nitrogen methyl pyrrolidone (NMP). The mixture was magnetically stirred for 24 hours. The resulting slurry was evenly coated on a copper foil. After vacuum drying at 120°C for 12 hours, the slurry was punched into 14 mm discs. The mass of the discs was weighed and subtracted from the mass of the blank copper foil to obtain the load mass (the load was 1 to 2 mg). The discs were then assembled into CR2032 button cells in a glove box protected by high-purity argon gas. The cells were allowed to stand for 8 hours before various electrochemical tests were performed.

[0012] In the above technical solution, the coal-based soft carbon precursor is anthracite, and the carbohydrate hard carbon precursor is sucrose.

[0013] In the above technical solution, the ratio of the carbohydrate hard carbon precursor to the coal-based soft carbon precursor is 3-6:4-7.

[0014] In the above technical solution, the atmosphere of the pretreatment carbonization step is one of air or argon.

[0015] In the above technical scheme, the washing steps of potassium hydroxide and hydrochloric acid solution are specifically as follows: the intermediate is placed in an agate mortar and fully ground, then dispersed into 300mL of 5mol / L potassium hydroxide solution, magnetically stirred at 70°C for 2 hours, and then filtered and washed with deionized water until pH≈7; then the intermediate is dispersed into a 5% hydrochloric acid solution prepared in advance, and magnetically stirred at 70°C for 2 hours.

[0016] In the method for preparing anthracite / sucrose-based composite carbon materials by two carbonizations described in the present invention, anthracite and sucrose will produce a cross-linking effect during the first low-temperature pretreatment process. The presence of anthracite will greatly inhibit the foaming behavior during the carbonization of sucrose, thereby improving the final carbon yield. At the same time, since the carbon material obtained after the carbonization of the anthracite-based precursor has a high conductivity and the sodium storage kinetics is mainly controlled by capacitance, the rate performance of the composite material can be improved and the long-cycle stability can be improved. The presence of sucrose can inhibit the ordering of microcrystals during the subsequent high-temperature carbonization process of anthracite, so that the composite carbon material has a suitable interlayer spacing, disorder and defect content, provides sodium storage sites, and ultimately makes the capacity higher than that of pure anthracite-based carbon materials. The simple dual impurity removal process of potassium hydroxide and hydrogen chloride can effectively remove most impurities, protect the material properties from the influence of impurities, and has good uniformity and stability, which is conducive to large-scale application.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The method for preparing anthracite / sucrose composite-based carbon materials by double carbonization described in the present invention utilizes a simple low-temperature pretreatment to first allow anthracite and sucrose to produce a cross-linking effect, then uses potassium hydroxide and hydrochloric acid to remove impurities in the raw materials, and finally carbonizes at 1200°C for a certain period of time to prepare a composite carbon material. The raw materials used are only anthracite and sucrose, which are widely available, low-priced, and environmentally friendly; the chemicals required for impurity removal, such as potassium hydroxide and hydrogen chloride, can also be well supplied.

[0019] The carbon material prepared by the method for preparing anthracite / sucrose-based composite carbon material by double carbonization described in the present invention is characterized by necessary microstructure. It is found that the material has a low impurity content after impurities are removed, has a reasonable microstructure, and has greatly improved performance. For example, the interlayer spacing in Example 1 is appropriate, the disorder is high, the defect content is rich, the equivalent series resistance is small, and the spectrum line in the low-frequency region is close to vertical, indicating that the ion diffusion resistance is small. At the same time, the electronic conductivity and ion conductivity of the material are both high, so it has good reversible specific capacity and cycle stability, and the rate performance is also excellent. It still has a specific capacity of 229mAh / g at a current density of 10C, and the capacity retention rate is 80% after 10C cycle 1300 times. These performance improvements indicate that the carbon material prepared by this method has broad commercial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The first three cycles of constant current charge-discharge curves of the anthracite / sucrose-based composite carbon material prepared in Example 1;

[0021] Figure 2 The rate performance of the anthracite / sucrose-based composite carbon material prepared in Example 1 in the current density range of 0.1C to 10C;

[0022] Figure 3 Cycling performance of the anthracite / sucrose-based composite carbon material prepared in Example 1 at a current density of 10C;

[0023] Figure 4 The AC impedance spectrum of the anthracite / sucrose-based composite carbon material prepared in Example 1 obtained at an open circuit voltage;

[0024] Figure 5 The rate performance of the anthracite / sucrose-based composite carbon material prepared in Example 2 in the current density range of 0.1C to 10C;

[0025] Figure 6 The cycle performance of the anthracite / sucrose-based composite carbon material prepared in Example 2 at a current density of 10C;

[0026] Figure 7 The rate performance of the anthracite / sucrose-based composite carbon material prepared in Example 3 in the current density range of 0.1C to 10C;

[0027] Figure 8 The cycle performance of the anthracite / sucrose-based composite carbon material prepared in Example 3 at a current density of 10C;

[0028] Fig. 9 This is the first cycle constant current charge and discharge curve of the anthracite / sucrose-based composite carbon material prepared in Example 4.

[0029] Fig.10 The constant current charge-discharge curves of the first three cycles of the sucrose-based hard carbon material prepared in Comparative Example 1;

[0030] Fig.11 The rate performance of the sucrose-based hard carbon material prepared in Comparative Example 1 in the current density range of 0.1C to 10C;

[0031] Fig.12 The cycling performance of the sucrose-based hard carbon material prepared in Comparative Example 1 at a current density of 10C;

[0032] Fig.13 The first three cycles of constant current charge and discharge curves of the anthracite-based soft carbon material prepared in Comparative Example 2;

[0033] Fig.14 The rate performance of the anthracite-based soft carbon material prepared in Comparative Example 2 in the current density range of 0.1C to 10C;

[0034] Fig.15 The cycle performance of the anthracite-based soft carbon material prepared in Comparative Example 2 at a current density of 10C;

[0035] Fig.16 XRD diffraction patterns of three different carbon materials prepared for Example 1, Comparative Example 1 and Comparative Example 2, wherein broad peaks of typical amorphous carbon materials appear near 2θ=26° and 43°, and the (002) interplanar spacings of different materials can be calculated according to the Bragg equation;

[0036] Fig.17 The Raman spectra of three different carbon materials prepared in Example 1, Comparative Example 1 and Comparative Example 2 show that D peak and G peak appear near 1350nm and 1580nm, and the peaks can be calculated by peak fitting of these two peaks. D / I G and I D4 / I G The value of

[0037] Fig.18The SEM images of three different carbon materials prepared in Example 1, Comparative Example 1 and Comparative Example 2, where the left side is the morphology of the sucrose-based hard carbon material prepared in Comparative Example 1, the middle is the morphology of the anthracite-based soft carbon material prepared in Comparative Example 2, and the right side is the morphology of the composite carbon material prepared in Example 1. It can be seen that the carbon materials prepared from different precursors have great differences in morphology;

[0038] Fig.19 The electronic conductivity of three different carbon materials prepared for Example 1, Comparative Example 1 and Comparative Example 2 was obtained by testing the powder samples by the four-probe method;

[0039] Fig. 20 The linear fitting diagrams of "square root of scan rate - peak current" of three different carbon materials were prepared for Example 1, Comparative Example 1 and Comparative Example 2. The peak current at the corresponding scan rate was found by measuring the cyclic voltammetry curves at different scan rates (0.2-5 mV / s). Finally, the peak current was obtained by plotting and fitting. According to the Rand les-Savcik formula: i p =269000n 2 / 3 ACD 1 / 2 v 1 / 2 It can be seen that the slope of the fitting line can reflect the diffusion coefficient of sodium ions in the material; DETAILED DESCRIPTION

[0040] The following will describe the implementation methods of the present application in detail with the help of accompanying drawings and examples, so that the implementation process of how the present application uses technical means to solve technical problems and achieve technical effects can be fully understood and implemented accordingly.

[0041] The invention provides a method for preparing anthracite / sucrose-based composite carbon material by double carbonization.

[0042] Example 1

[0043] According to the mass ratio of sucrose to anthracite of 3:7, weigh sucrose and anthracite raw materials in a ball mill, and use alcohol as the ball milling solvent. Ball mill for 12 hours to fully mix the raw materials; then dry them in an oven at 80°C for 12 hours; transfer the dried raw materials to a corundum crucible, and then place them in a tubular atmosphere furnace, continuously introduce argon, and after the air in the furnace is exhausted, heat it to 400°C at a heating rate of 5°C / min, keep it warm for 2 hours, and then naturally cool it to room temperature with the furnace, close the air inlet valve and stop introducing argon. The intermediate is ground with an agate mortar for 15 minutes, then poured into a 300mL 5M KOH solution prepared in advance, and magnetically stirred at 70°C for 2 hours, then filtered and washed to remove excess alkali solution, and then dispersed in 300mL 5% HCl solution, magnetically stirred at 70°C for 2 hours, and then filtered and washed until the pH value of the solution is approximately equal to 7. Finally, after drying at 120°C for 12 hours, it was placed in a tubular atmosphere furnace, heated to 1200°C at 5°C / min under an argon protective atmosphere, and naturally cooled to room temperature after carbonization for 2 hours to obtain anthracite / sucrose-based composite carbon material. Then, electrode sheets were prepared to assemble button batteries. The specific electrode sheet preparation process was as follows: 0.9g and 0.05g of sample and conductive carbon (Super P li) were weighed in an agate mortar, ground for 15 minutes and mixed evenly, then transferred to a 20mL sampling bottle, and 1g of NMP solution containing 5% PVDF was added. At this time, sample: conductive carbon: PVDF = 90:5:5; finally, an appropriate amount of NMP solution was added to adjust the slurry consistency, magnetically stirred for 24 hours, and then evenly coated on copper foil, and vacuum dried at 120°C for 12 hours, punched into discs with a diameter of 14mm, assembled into button batteries in a glove box and waited for testing. The electrochemical test voltage range is 0-2.5V, and the capacity is measured at a current density of 0.1C (30mA / g). When testing the rate performance, the current density changes continuously from 0.1C to 10C, and then returns to a low current density. The cycle stability is judged based on the electrochemical performance after 1300 cycles at a high current density (10C). It is worth noting that all specific capacity values ​​in this patent are calculated based on the overall load mass, which includes the mass of the active material, binder and conductive carbon.

[0044] like Figure 1As shown, the composite carbon material prepared in Example 1 exhibits a charge and discharge curve similar to that of hard carbon, that is, there is an obvious charge and discharge platform below 0.1V. At 0.1C, the first discharge specific capacity is 344.7mAh / g, the first charge specific capacity is 271.8mAh / g, and the first coulombic efficiency calculated by dividing the charge specific capacity by the discharge specific capacity is 78.85%. The first cycle of charge and discharge has an irreversible capacity of 72.9mAh / g. This is because part of the electrolyte is consumed to form the SE I film. After a uniform and stable SE I film is formed, the carbon anode material can be stably charged and discharged without obvious irreversible losses. Therefore, the charge and discharge curves of the last two cycles overlap well. Figure 2 As shown, the anthracite / sucrose-based composite carbon anode prepared in this embodiment has excellent rate performance and can maintain a specific capacity of 229 mAh / g even at a high current density of 10C. Figure 3 This shows that the material has good cycle stability. After 1300 cycles at a high current density of 10C, it still has a specific capacity of 188mAh / g, and the capacity retention rate is 80%. Figure 4 This is the AC impedance diagram of the sample in this embodiment. The equivalent series resistance of the material is small, only 4Ω; there is no obvious semicircular area, indicating that the charge transfer impedance is very small; the slope of the spectrum line in the low-frequency region is related to the diffusion rate of ions in the solid phase. It can be seen from the figure that the slope of the spectrum line in the low-frequency region is large, basically close to vertical, indicating that the ion diffusion impedance is also small and the material performance is good.

[0045] Example 2

[0046] The raw materials, preparation steps and process conditions used in this embodiment are the same as those in Example 1, and the test conditions and instruments used are also the same, except that the ratio of sucrose to anthracite is changed, that is, the composite carbon material is prepared according to a ratio of sucrose to anthracite of 4:6.

[0047] The rate performance of the composite carbon material of this embodiment in the current density range of 0.1-10C was tested under the same test conditions as in Example 1. Figure 5 As shown, the initial specific capacity is 180.0 mAh / g, and at 10C it is 140.8 mAh / g, which is lower than 229 mAh / g in Example 1. After 1300 cycles at 10C, only 146 mAh / g remains ( Figure 6 ), indicating that the rate performance and cycle performance of this embodiment are not as good as those of embodiment 1.

[0048] Example 3

[0049] The raw materials, preparation steps and process conditions used in this embodiment are the same as those in Example 1, and the test conditions and instruments used are also the same, except that the ratio of sucrose to anthracite is changed, that is, the composite carbon material is prepared according to a ratio of sucrose to anthracite of 6:4.

[0050] The rate performance of the composite carbon material of this embodiment in the current density range of 0.1-10C was tested under the same test conditions as in Example 1, and the results are as follows: Figure 7 As shown, the initial capacity of the composite material prepared in this embodiment is 204.1 mAh / g, and it has a specific capacity of 156.1 mAh / g at 10C; after 10C cycle 1300 times, it has only a specific capacity of 119 mAh / g ( Figure 8 ), which is lower than 188 mAh / g of Example 1. This shows that the composite ratios of Examples 2 and 3 are not the best composite ratios, and when the materials are composited at a ratio of 3:7, the cross-linking effect of sucrose and anthracite is most sufficient, which can maximize the synergistic effect of soft carbon and hard carbon, and make the material have the best performance.

[0051] Example 4

[0052] The raw materials and preparation steps used in this example are the same as those in Example 1, except that the 400°C pretreatment step is carried out in air without the introduction of protective gas. This step is a pre-oxidation process that serves to introduce more oxygen atoms into the precursor. The subsequent process conditions are the same as those in Example 1, and the test conditions and instruments used are also the same. Fig. 9 As shown, the reversible capacity of the sample pretreated in air at 0.1C is only 190.8 mAh / g, and the first coulombic efficiency is only 72.35%, which is lower than that of Example 1, indicating that argon is more suitable for the pretreatment atmosphere. Increasing the oxygen content of the material will reduce the reversible specific capacity and the first coulombic efficiency.

[0053] Comparative Example 1

[0054] The preparation steps and process conditions used in this comparative example are the same as those in Example 1, but only sucrose is used as the raw material without adding anthracite, so the obtained carbon material is a typical sucrose-based hard carbon material. The test conditions and instruments used for the experimental results in this comparative example are also the same as those in Example 1.

[0055] The capacity, rate performance and cycle performance of the hard carbon of Comparative Example 1 were tested under the same test conditions as in Example 1. Fig.10 As shown, the first discharge capacity of the sucrose-based hard carbon material is 357.2 mAh / g, and the first charge capacity is 279.7 mAh / g, which is not much different from the composite carbon material in Example 1. Fig.11 It can be seen that its rate performance is poor, with only 23.8 mAh / g of specific capacity retained at 10C, which obviously cannot meet the requirements of practical applications. Fig.12 This indicates that the capacity of the material in this example decays rapidly in a 10C high current long cycle, with only 90 mAh / g remaining after 1300 cycles.

[0056] Comparative Example 2

[0057] The preparation steps and process conditions used in this comparative example are the same as those in Example 1, but only anthracite is used as the raw material, and sucrose is not added, so the obtained carbon material is similar to anthracite-based soft carbon material. The test conditions and instruments used for the experimental results in this comparative example are also the same as those in Example 1. Fig.13 As shown in the figure, the charge and discharge curve of anthracite-based carbon material is a sloping curve, and there is no obvious charge and discharge platform below 0.1V, indicating that the material tends to be soft carbon, so its specific capacity is low, with only 178.2mAh / g reversible capacity at 0.1C. The large number of defects on the surface of soft carbon lead to its irreversible capacity of 105.4mAh / g, and the first charge and discharge efficiency is only 62.83%. However, due to the high conductivity of anthracite-based carbon material and the sodium storage mechanism is mainly controlled by surface capacitance, its rate performance is better than that of sucrose-based hard carbon material in Comparative Example 1, such as Fig.14 As shown, it is 118 mAh / g at a high current density of 10C. Fig.15 It is the long cycle performance of the carbon material in this comparative example. It can stably cycle 1100 times at a current density of 10C and has a reversible specific capacity of 165mAh / g. However, after 1100 cycles, the material can no longer withstand large current charging and discharging, and the battery is difficult to continue to charge and discharge stably.

[0058] The carbon materials prepared in Example 1, Comparative Sample 1 and Comparative Sample 2 were tested by X-ray diffractometer to obtain Fig.16 The XRD spectrum shown in the figure has broad peaks at 2θ=26° and 43°, indicating that the prepared carbon material is a typical amorphous carbon material. The interlayer spacing of the (002) crystal plane of different carbon materials is calculated according to the Bragg equation. The composite carbon material in Example 1 is 0.3707nm, the sucrose-based hard carbon material in Comparative Example 1 is 0.3783nm, and the soft carbon-based carbon material prepared in Comparative Example 2 is 0.3688nm. A sharper diffraction peak appears at the edge of the broad peak, which corresponds well to the diffraction peak position of graphene. This indicates that a crystalline phase may appear locally in the amorphous phase material, further proving that the carbon material obtained only by carbonization of anthracite has a low degree of disorder, which is not conducive to the storage of sodium ions. The interlayer spacing of sucrose after carbonization is the largest, which is conducive to the interlayer embedding process of sodium ions, so the capacity is the highest, while the composite carbon material d (002) The value is between the two, indicating that the two precursors can influence each other during the composite process to generate a carbon material with a different structure from that of a single precursor after carbonization.

[0059] Fig.17 The RAMAN spectra of Example 1 and Comparative Samples 1 and 2 are deconvoluted into five peaks: G, D1, D2, D3, and D4. I D / I G and ID4 / I G The value of I D / I G It can reflect the disorder of the material. D4 / I G It can reflect the number of defective functional groups. D / I G is 2.59, I D4 / I G is 0.65, and the I of the pure anthracite-based carbon material prepared in Comparative Example 2 D / I G and I D4 / I G 2.57 and 0.60 respectively, while the I of the composite carbon material prepared in Example 1 D / I G is 3.07, I D4 / I G It is 0.94, which is obviously higher than the two groups of comparative samples. This shows that the composite material has the highest degree of disorder and contains the most defective functional groups such as edges. Such a structure is conducive to the rapid storage of sodium ions.

[0060] Fig.18 The scanning electron microscope images of Comparative Example 1, Comparative Example 2 and Example 1 show that the sucrose-based carbon material (left) is granular and has a relatively smooth surface, while the anthracite carbon material (middle) shows more flaky features and a rough surface. The flaky morphology is conducive to increasing the contact area with the electrolyte, accelerating the sodium storage dynamics, and improving the rate performance of the material. The morphology of the anthracite / sucrose-based composite carbon material (right) is a cluster of particles and flaky particles, with a rough surface. At the same time, the composite material contains more edges, protrusions and holes, etc. These structural features are conducive to the rapid storage process of sodium ions, so the sucrose / anthracite-based composite material has the best rate performance. The above series of structural characterizations can explain that sucrose and anthracite have a specific cross-linking effect in the composite process. With the help of effective potassium hydroxide and hydrochloric acid impurity removal steps, the interlayer spacing, disorder, defect content and morphology of the carbon material can be effectively adjusted, and finally the composite carbon material has both the high capacity of hard carbon and the good rate performance and cycle stability of soft carbon.

[0061] Fig.19 The electronic conductivity of Comparative Examples 1 and 2 and Example 1 tested by an intelligent powder resistivity tester.

[0062] Fig. 20 is the peak current of the three -v 1 / 2The linear fitting graph shows that the slope of the fitting curve can reflect the diffusion coefficient of sodium ions in the material. The anthracite has a high degree of order in the microcrystals after carbonization, and the flaky morphology increases the contact area with the electrolyte, so its electronic conductivity and ionic conductivity are both high. The carbon material after sucrose carbonization has a large degree of disorder and rich defects, resulting in low electronic conductivity. The granular morphology is not conducive to the diffusion of sodium ions, so the ionic conductivity is also low. The composite of sucrose and anthracite and the alkali and acid impurity removal process can effectively adjust the degree of disorder, interlayer spacing and morphology of the microcrystals. The flaky morphology characteristics and abundant edges and holes are conducive to the diffusion and rapid storage of sodium ions in the electrode material. Therefore, the composite material has high electronic conductivity and ionic conductivity, and has a high specific capacity while improving the rate performance and cycle stability. In summary, the composite of sucrose and anthracite can overcome the shortcomings of a single precursor that it is difficult to have both high capacity and good rate performance and cycle stability. The cross-linking reaction of the two precursors can be used to exert the synergistic effect of soft and hard carbon, so that the composite carbon material has a higher specific capacity and excellent performance in rate performance and cycle stability. This composite strategy has great potential for commercial application.

[0063] Among the raw materials used, anthracite was produced in Hunyuan County, Datong City, Shanxi Province, sucrose and sodium hydroxide were purchased from Chengdu Zhuopu Instrument Co., Ltd., and hydrochloric acid was purchased from Chengdu Kelong Chemicals Co., Ltd.

[0064] The instruments, utensils and equipment used include planetary ball mill (QM-3SP2), vacuum drying oven (DZF-6020AB), OTF-1200X tubular atmosphere furnace, agate mortar, corundum crucible, protective gas cylinder, DF-101S collector constant temperature heating magnetic stirrer, small hydraulic button battery disassembly machine (MSK-110D); DX-1000 X-ray diffractometer, CHI-660E electrochemical workstation, scanning electron microscope (SEM, Apreo S type); Raman (LabRAM HR), blue battery test system (CT3002), intelligent powder resistivity tester (FT-301B), TALD-41R glove box (Jiaxing Kemin Electronic Equipment Technology Co., Ltd., Shanghai Mikaelona Electromechanical Technology Co., Ltd.);

[0065] The electrochemical tests of each embodiment were conducted after being assembled into a CR2032 button cell, with glass fiber (Whatman, GF / D) as the electrolytic diaphragm, 1 mol sodium hexafluorophosphate (NaPF6) dissolved in 1 liter of ethylene glycol dimethyl ether (DME) as the electrolyte, and metallic sodium as the counter electrode.

[0066] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the present invention in any form. Any simple modifications or equivalent changes made to the above embodiments based on the technical essence of the present invention fall within the protection scope of the present invention.

[0067] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention are within the scope of the technical solution of the present invention.

Claims

1. A method for preparing anthracite / sucrose-based composite carbon material by double carbonization, characterized in that: The following steps are involved: S1. Weigh the coal-based soft carbon precursor and the carbohydrate hard carbon precursor in different proportions, then ball-mill the two raw materials to mix them evenly, and then dry them; S2, transferring the mixed powder obtained in step S1 to a tubular furnace, heating it under an atmosphere, and keeping it warm, and then naturally cooling it to room temperature with the furnace, thus completing the first pretreatment carbonization step and obtaining an intermediate; S3, washing the intermediate obtained in step S2 with potassium hydroxide and hydrochloric acid solution in sequence to remove impurities, washing with deionized water until neutral, and then drying in an oven; S4, transferring the intermediate after impurity removal and drying in step S3 to a tubular furnace, heating it under the protection of an inert gas and keeping it warm for 2 hours, and then cooling it to room temperature with the furnace, thereby preparing a composite carbon material; S5. Dissolve the carbon material, conductive carbon and binder in nitrogen-methyl pyrrolidone and stir magnetically for 24 hours. Evenly coat the obtained slurry on copper foil and dry it in vacuum at 120°C for 12 hours. Then take out the slurry and punch it into 14 mm discs. Weigh the mass of the discs and subtract it from the mass of the blank copper foil to get the load mass (the load is 1-2 mg). Then assemble it into CR2032 button batteries in a glove box protected by high-purity argon gas and perform various electrochemical tests after standing for 8 hours.

2. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: In step S1, the ball milling time is 12 hours, the drying time is 12 hours, and the drying temperature is 80°C. In step S2, the temperature is increased to 400°C at a heating rate of 5°C / min and the heat preservation time is 2 hours. In step S4, the temperature is increased to 1200°C at a heating rate of 5°C / min and the heat preservation time is 2 hours.

3. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: In step S3, the concentration of potassium hydroxide is 5M, the dilution of the hydrochloric acid solution is 5%, and in step S3, after washing, the oven temperature is 120°C and the drying time is 12 hours.

4. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: In step S2, the atmosphere is one of air and argon.

5. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: In step S4, the inert gas is argon.

6. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: In step S5, the mass ratio of carbon material, conductive carbon (Super P li) and binder (PVDF) is 90:5:

5.

7. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: The coal-based soft carbon precursor is anthracite, and the carbohydrate hard carbon precursor is sucrose.

8. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to any one of claims 1 or 7, characterized in that: The ratio of the carbohydrate hard carbon precursor to the coal-based soft carbon precursor is 3-6:4-7.

9. The method for preparing anthracite / sucrose-based composite carbon material by double carbonization according to claim 1, characterized in that: The potassium hydroxide and hydrochloric acid solution washing steps are specifically as follows: the intermediate is placed in an agate mortar and fully ground, then dispersed into 300 mL of a 5 mol / L potassium hydroxide solution, magnetically stirred at 70° C. for 2 hours, then filtered and washed with deionized water until the pH is approximately 7; then the intermediate is dispersed into a 5% hydrochloric acid solution prepared in advance, and magnetically stirred at 70° C. for 2 hours.

10. Use of an anthracite / sucrose-based composite carbon material prepared by the method for preparing anthracite / sucrose-based composite carbon material by double carbonization as described in any one of claims 1 to 9 in a sodium ion battery.

Citation Information

Patent Citations

  • Hard carbon material for anode of sodium-ion battery, preparation method of hard carbon material and related sodium-ion battery

    CN109678130A

  • Sodium ion total battery and preparation method thereof

    CN111063871A

  • Amorphous carbon negative electrode material and preparation method and application thereof

    CN115881895A

  • High-performance hard carbon negative electrode material for high-temperature sodium-ion battery and preparation method of high-performance hard carbon negative electrode material

    CN116040605A

  • Sodium ion secondary battery anode material and preparing method and application thereof

    US20190006673A1

Cited By

  • Coal-based carbon negative electrode material, preparation method thereof and full-carbon-based lithium ion capacitor

    CN121282016A

  • Sucrose-polymer composite hard carbon and preparation method thereof

    CN122276705A