Preparation method of magnetic nitrogen-doped porous carbon aerogel wave-absorbing material
FeNi10@NCA magnetic nitrogen-doped porous carbon aerogels were prepared through ultrasound-assisted self-crosslinking reaction and in-situ impregnation of metal salts, which solved the problems of high density and narrow absorption bandwidth of existing absorbing materials and achieved high The preparation of high-performance, lightweight and multi-functional electromagnetic wave absorbing materials is suitable for industrial production and complex environments.
Patent Information
- Application Number
- CN202411021776.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-29
AI Technical Summary
Existing electromagnetic wave absorbing materials have high density, narrow effective absorption bandwidth, large thickness, poor absorption strength, complex preparation process and are not suitable for industrial production. Moreover, the dispersion of magnetic particles in the gel is poor, which affects the absorption performance.
COF hydrogel was prepared using ultrasound-assisted self-crosslinking reaction, and was immersed in a metal salt solution in situ. After freeze-drying and pyrolysis treatment, FeNi10@NCA magnetic nitrogen-doped porous carbon aerogel was formed to achieve uniform magnetic particles. Preparation of dispersion and high performance absorbing materials.
A lightweight, stable, and uniform particle magnetic porous carbon aerogel was obtained, which has excellent electromagnetic wave absorption capabilities, a reflection loss value of -63.8 dB, and a wide bandwidth, making it suitable for multi-scenario applications.
Smart Images

Figure CN118754102A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material, and specifically belongs to the technical field of electromagnetic wave absorbing materials. Background Art
[0002] The rapid development of wireless technology has improved our quality of life, but the widespread use of wireless electronic devices has inevitably led to serious electromagnetic wave pollution, which is considered to be the fourth largest source of pollution after air, water and noise pollution. Therefore, it is urgent to find a feasible way to solve the problem of electromagnetic wave pollution. At present, aerogel materials based on graphene and biomass are considered to be a promising candidate for electromagnetic wave absorption due to their advantages of light weight and porosity. However, the preparation conditions of graphene aerogel are harsh and the process is complicated, and the wave absorption performance of biomass aerogel is unstable. Both are difficult to meet the needs of actual production.
[0003] Patent "A novel method for preparing three-dimensional porous biomass-derived carbon aerogel" (CN 117756093A): Tofu is used as raw material, and three-dimensional porous biomass-derived carbon aerogel is obtained after heat treatment. Although this method is relatively simple, its wave absorption performance is poor. When the matching thickness is 3.38 mm, the minimum reflection loss value ( RL min ) is -57.23 dB, and biomass materials often have unclear components and contain impurities, with poor performance reproducibility, making it difficult to apply them in more complex and changeable environments. Patent "A nitrogen-doped graphene aerogel absorbing material and its preparation method" (CN 118062833A): First, a nitrogen source is added to an aqueous solution of graphene oxide to prepare a nitrogen-doped graphene hydrogel, and the nitrogen-doped graphene hydrogel is dialyzed and freeze-dried to obtain a nitrogen-doped graphene aerogel absorbing material. This method requires the addition of a nitrogen source as a gelling aid, which makes it difficult to spontaneously form a hydrogel in situ. And due to the lack of magnetic loss, when the coating thickness is 1.62 mm, RL min It can only reach -28.3 dB. Patent "A method for preparing a cobalt-nickel / graphite-phase carbon nitride / reduced graphene oxide composite aerogel absorber" (CN 116456707A): First, cobalt-nickel magnetic nano-metal particles and graphite-phase carbon nitride are obtained by solvent thermal and thermal polymerization methods, respectively, and then cobalt-nickel magnetic metal nano-particles, graphite-phase carbon nitride, and graphene oxide are mixed by a one-pot hydrothermal method to obtain a hydrogel of the composite material, and finally freeze-dried and thermally annealed to obtain a cobalt-nickel / graphite-phase carbon nitride / reduced graphene oxide composite aerogel. This method is cumbersome to prepare and has harsh conditions. It is difficult to meet the requirements of industrial production and practical applications, and the added magnetic particles cannot obtain good electromagnetic wave absorption due to problems such as agglomeration. At present, aerogel absorbers need to be further improved in terms of preparation methods and stability of absorbing performance.
[0004] Compared with other traditional porous materials such as molecular sieves, porous polymers, metal organic frameworks (MOFs), the emerging porous covalent organic frameworks (COFs) have the following characteristics: 1. COFs are orderly connected by strong covalent bonds, so they have good thermal stability and chemical stability; 2. Ultra-large specific surface area and adjustable pore channels, different network structures can be constructed through different building blocks and connection methods; 3. Designability of composition and pore size. However, most COF absorbing materials still have problems such as cumbersome synthesis process, high preparation cost, and easy environmental pollution during the production process, which hinders the further widespread application of advanced absorbing materials. In order to make full use of its structural advantages, the present invention designs COF-derived porous carbon aerogels with high specific surface area and low density, which provides a simple, practical and innovative method for preparing nitrogen-doped porous carbon aerogels.
[0005] It is worth noting that it is still challenging to achieve broadband absorption in a single carbon material, so introducing magnetic components into carbon materials to optimize impedance and broaden bandwidth is a visionary strategy. However, directly adding magnetic particles to the gel will cause the magnetic particles to aggregate or deposit at the bottom of the gel, and good dispersion cannot be achieved, which is not conducive to the formation of magnetic aerogels. Therefore, it is still a very challenging task to develop a simple and sustainable preparation method to achieve uniform dispersion of magnetic particles in aerogels to obtain high-performance, multifunctional magnetic porous carbon aerogels. Summary of the invention
[0006] The present invention aims to solve the problems of high density, narrow effective absorption bandwidth, large thickness and poor absorption intensity of current absorbing materials, and provides a simple preparation method of magnetic COF-derived nitrogen-doped porous carbon aerogel absorbing material.
[0007] The present invention discloses a method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material. The method comprises the following steps: obtaining a COF hydrogel by an ultrasound-assisted self-crosslinking reaction under the action of a scandium trifluoromethanesulfonate catalyst, in-situ immersing a metal salt solution into the COF hydrogel, and then freeze-drying and externally heat-dried to obtain a magnetic nitrogen-doped porous carbon aerogel absorbing material. The specific steps are as follows: Step 1: Add terephthalaldehyde, 1,3,5-tri(4-aminophenyl)benzene and scandium trifluoromethanesulfonate (Sc(OTf)3) to N,N-dimethylformamide, and after ultrasound-assisted self-crosslinking reaction, stand and crystallize to form COF gel, and then use N,N-dimethylformamide, acetone, ethanol, methanol and water to exchange solvents in sequence to obtain COF hydrogel; Step 2: Add nickel (II) chloride hexahydrate and iron (III) chloride hexahydrate solution to the COF hydrogel to allow the metal ions to be in situ immersed in the hydrogel, followed by freeze drying overnight to obtain FeNi10 @COF aerogel; Step 3: calcining and pyrolyzing the COF aerogel under a protective gas atmosphere to obtain FeNi 10 @NCA aerogel, that is, magnetic nitrogen-doped porous carbon aerogel absorbing material.
[0008] In the step 1, the ratio of terephthalaldehyde, 1,3,5-tris(4-aminophenyl)benzene, scandium trifluoromethanesulfonate and N,N-dimethylformamide is 0.0134-0.0268 g: 0.0234-0.0468 g: 0.05-0.1 g: 4 mL, and the ultrasound-assisted self-crosslinking reaction time is 5-10 minutes.
[0009] In the step 2, the ratio of nickel (II) chloride hexahydrate to iron (III) chloride hexahydrate is 0.0862-0.3457 g: 0.0098-0.0393 g.
[0010] In the step 3, the protective gas is nitrogen or argon, the calcination and pyrolysis temperature is 600-900°C, the temperature is kept for 2-3 hours, and the heating rate is 2-3°C / min.
[0011] Beneficial effects of the present invention: 1. Unique preparation method: The present invention adopts ultrasound-assisted COF self-crosslinking reaction and metal salt in-situ impregnation method to successfully design a FeNi 10 Electromagnetic functional composite material composed of alloy nanoparticles and N-doped porous carbon aerogel (NCA). Under the action of scandium trifluoromethanesulfonate catalyst, COF gel can be directly obtained within five minutes through self-crosslinking reaction. After metal salt impregnation, metal ions are uniformly adsorbed in the porous channels of COF hydrogel. After further freeze drying and calcination pyrolysis, ultralight magnetic porous carbon aerogel is obtained. The preparation process of the present invention is simple, the reliability is high, the material has excellent stability, uniform particles, light weight and strong absorption capacity.
[0012] 2. Excellent electromagnetic wave absorption ability: FeNi 10 @NCA aerogel material has the best reflection loss value at 2.09 mm ( RL min ) can reach -63.8 dB. Moreover, only 10 wt.% of aerogel material in the paraffin matrix can obtain an ultra-wide absorption bandwidth of 6.56 GHz, and the matching thickness is only 2.28 mm, which meets the requirements of "thin, light, wide and strong" for ideal absorbing materials, which has great potential for industrial production and application.
[0013] 3. Applicability in multiple scenarios: Multifunctional performance makes up for the disadvantage of single material application scenario. At the same time, the multifunctionalization of materials is also the development trend of future metamaterials. Aerogel has excellent thermal insulation performance, excellent radar stealth performance and excellent absorption bandwidth. Therefore, magnetic COF-derived nitrogen-doped porous carbon aerogel is suitable for practical applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 : X-ray diffraction patterns of magnetic nitrogen-doped porous carbon aerogel absorbing materials prepared in Examples 1, 2, 3 and 4 of the present invention; Figure 2 : Scanning electron microscopic image of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention; Figure 3 : Transmission electron micrograph of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention; Figure 4a : Nitrogen adsorption-desorption isotherms of magnetic nitrogen-doped porous carbon aerogel absorbing materials prepared in Examples 1, 2, 3 and 4 of the present invention; Figure 4b : Pore size distribution curves of magnetic nitrogen-doped porous carbon aerogel absorbing materials prepared in Examples 1, 2, 3 and 4 of the present invention; Figure 5 : Vibrating sample magnetometer (VSM) images of magnetic nitrogen-doped porous carbon aerogel absorbing materials prepared in Examples 1, 2, 3 and 4 of the present invention; Figure 6a : Electromagnetic wave absorption diagram of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 1 of the present invention; Figure 6b : Electromagnetic wave absorption diagram of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 2 of the present invention; Figure 6c : Electromagnetic wave absorption diagram of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention; Figure 6d : Electromagnetic wave absorption diagram of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 4 of the present invention; Figure 7a : Temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention at 0 minutes; Figure 7b : The temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention for 10 minutes; Figure 7c: Temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention for 20 minutes; Figure 7d : Temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention for 30 minutes; Figure 7e : Temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention for 40 minutes; Figure 7f : Temperature diagram of the thermal insulation test of the magnetic nitrogen-doped porous carbon aerogel absorbing material prepared in Example 3 of the present invention for 60 minutes. DETAILED DESCRIPTION
[0017] Example 1 Step 1: In a glass bottle containing 4 mL of N,N-dimethylformamide, 0.0268 g of terephthalaldehyde, 0.01 g of scandium trifluoromethanesulfonate and 0.0468 g of 1,3,5-tri(4-aminophenyl)benzene were added in sequence, and then the mixture was ultrasonicated until uniform. After ultrasonication for 5 min, it was allowed to stand and crystallize to form a COF gel. The formed COF gel was solvent exchanged with N,N-dimethylformamide, acetone, ethanol, methanol and water in sequence, and the solvent was exchanged 2 to 3 times each time. The last time, the water solvent was exchanged 4 to 5 times to obtain a COF hydrogel.
[0018] Step 2: Dissolve 0.0861 g of nickel chloride hexahydrate and 0.0098 g of ferric chloride hexahydrate in 4 mL of deionized water, add the salt solution of nickel chloride hexahydrate and ferric chloride hexahydrate to the COF hydrogel in step 1, and the nickel and iron metal ions in the solution are adsorbed by the porous structure of the COF hydrogel. Let it stand for 4 to 5 days until the solution becomes colorless. Then freeze-dry overnight to obtain FeNi 10 @COF aerogel.
[0019] Step 3: FeNi 10 @COF aerogel was placed on a quartz boat and moved into a tube furnace. The temperature was kept at 800℃ in a nitrogen atmosphere for 2 h at a heating rate of 2℃min -1 , calcined and pyrolyzed to obtain FeNi 10 @NCA-1 aerogel, that is, magnetic nitrogen-doped porous carbon aerogel absorbing material.
[0020] Step 4: Place the petals on the prepared FeNi 10 @NCA-1 aerogel, heated by alcohol lamp, and the changes of petals were recorded with a mobile phone. After heating by alcohol lamp for 0, 30, 60, and 120 seconds, the shape of petals did not change significantly, proving that the aerogel has good thermal insulation performance.
[0021] Step 5: Use CST electromagnetic field simulation software to simulate the FeNi 10 The radar stealth performance of @NCA-1 aerogel is simulated, and the calculation formula of its radar cross-section is as follows: ;
[0022] Step 6: Prepare FeNi 10 @NCA-1 Aerogel Aerogel material is immersed in melted paraffin as a substrate and made into a ring. The density of the aerogel is calculated to obtain that the material accounts for 10 wt.% of the total mass of the ring. The electromagnetic parameters of the material are measured by a vector network analyzer. According to the transmission line theory, the calculation formula for the reflection loss of the material to the electromagnetic wave is as follows: .
[0023] Example 2 Step 1: In a glass bottle containing 4 mL of N,N-dimethylformamide, 0.0268 g of terephthalaldehyde, 0.01 g of scandium trifluoromethanesulfonate and 0.0468 g of 1,3,5-tri(4-aminophenyl)benzene were added in sequence, and then the mixture was ultrasonicated until uniform. After ultrasonication for 5 min, it was allowed to stand and crystallize to form a COF gel. The formed gel was solvent exchanged with N,N-dimethylformamide, acetone, ethanol, methanol and water in sequence, and the solvent was exchanged 2 to 3 times each time. The last time, the water solvent was exchanged 4 to 5 times to obtain a COF hydrogel.
[0024] Step 2: Dissolve 0.1728 g of nickel chloride hexahydrate and 0.0197 g of ferric chloride hexahydrate in 4 mL of deionized water, add the salt solution of nickel chloride hexahydrate and ferric chloride hexahydrate to the COF hydrogel in step 1, and the nickel and iron metal ions in the solution are adsorbed by the porous structure of the COF hydrogel. Let it stand for 4 to 5 days until the solution becomes colorless. Then freeze-dry overnight to obtain FeNi 10 @COF aerogel.
[0025] Step 3: FeNi 10 @COF aerogel was placed on a quartz boat and moved into a tube furnace. The temperature was kept at 800℃ in a nitrogen atmosphere for 2h at a heating rate of 2℃min -1 , calcined and pyrolyzed to obtain FeNi 10 @NCA-2 aerogel, that is, magnetic nitrogen-doped porous carbon aerogel absorbing material.
[0026] Step 4: Place the petals on the prepared FeNi 10 @NCA-2 aerogel, heated by alcohol lamp, and the changes of petals are recorded with a mobile phone.
[0027] Step 5: Use CST electromagnetic field simulation software to simulate the FeNi 10The radar stealth performance of @NCA-2 aerogel is simulated, and the calculation formula of its radar cross-section is as follows: ; Step 6: Prepare FeNi 10 @NCA-2 aerogel material was immersed in melted paraffin as a substrate and made into a ring. The density of the aerogel was calculated to obtain that the material accounted for 10 wt.% of the total mass of the ring. The electromagnetic parameters of the material were measured by a vector network analyzer. According to the transmission line theory, the calculation formula for the reflection loss of the material to the electromagnetic wave is as follows: .
[0028] Example 3 Step 1: In a glass bottle containing 4 mL of N,N-dimethylformamide, 0.0268 g of terephthalaldehyde, 0.01 g of scandium trifluoromethanesulfonate and 0.0468 g of 1,3,5-tri(4-aminophenyl)benzene were added in sequence, and then the mixture was ultrasonicated until uniform. After ultrasonication for 5 min, it was allowed to stand and crystallize to form a COF gel. The formed gel was solvent exchanged with N,N-dimethylformamide, acetone, ethanol, methanol and water in sequence, and the solvent was exchanged 2 to 3 times each time. The last time, the water solvent was exchanged 4 to 5 times to obtain a COF hydrogel.
[0029] Step 2: Dissolve 0.2593 g of nickel chloride hexahydrate and 0.0.0295 g of ferric chloride hexahydrate in 4 mL of deionized water, add the salt solution of nickel chloride hexahydrate and ferric chloride hexahydrate to the COF hydrogel in step 1, and the nickel and iron metal ions are adsorbed by the porous structure of the COF hydrogel. Let it stand for 4 to 5 days until the solution becomes colorless. Then freeze-dry overnight to obtain FeNi 10 @COF aerogel.
[0030] Step 3: FeNi 10 The @COF aerogel was placed on a quartz boat and moved into a tubular furnace. It was calcined and pyrolyzed at 800 °C in a nitrogen atmosphere for 2 h at a heating rate of 2 °C / min to obtain FeNi@NCA-3 aerogel.
[0031] Step 4: Place the petals on the prepared FeNi 10 @NCA-3 aerogel, heated by alcohol lamp, and the changes of petals recorded with mobile phone.
[0032] Step 5: Use CST electromagnetic field simulation software to simulate the FeNi 10 The radar stealth performance of @NCA-3 aerogel is simulated, and the calculation formula of its radar cross-section is as follows: ; Step 6: Prepare FeNi10 @NCA-3 aerogel material was immersed in melted paraffin as a substrate and made into a ring. The density of the aerogel was calculated to obtain that the material accounted for 10 wt.% of the total mass of the ring. The electromagnetic parameters of the material were measured by a vector network analyzer. According to the transmission line theory, the calculation formula for the reflection loss of the material to the electromagnetic wave is as follows: .
[0033] Example 4 Step 1: In a glass bottle containing 4 mL of N,N-dimethylformamide, 0.0268 g of terephthalaldehyde, 0.01 g of scandium trifluoromethanesulfonate and 0.0468 g of 1,3,5-tri(4-aminophenyl)benzene were added in sequence, and then the mixture was ultrasonicated until uniform. After ultrasonication for 5 min, it was allowed to stand and crystallize to form a COF gel. The formed COF gel was solvent exchanged with N,N-dimethylformamide, acetone, ethanol, methanol and water in sequence, and the solvent was exchanged 2 to 3 times each time. The last time, the water solvent was exchanged 4 to 5 times to obtain a COF hydrogel.
[0034] Step 2: Dissolve 0.3457 g of nickel chloride hexahydrate and 0.0393 g of ferric chloride hexahydrate in 4 mL of deionized water, add the salt solution of nickel chloride hexahydrate and ferric chloride hexahydrate to the gel in step 1, and the nickel and iron metal ions are adsorbed by the porous structure of the COF hydrogel. Let it stand for 4 to 5 days until the solution becomes colorless. Then freeze-dry overnight to obtain FeNi@COF aerogel.
[0035] Step 3: FeNi 10 @COF aerogel was placed on a quartz boat and moved into a tube furnace. The temperature was kept at 800℃ in a nitrogen atmosphere for 2h at a heating rate of 2℃min -1 , FeNi@NCA-4 aerogel was prepared by pyrolysis.
[0036] Step 4: Place the petals on the prepared FeNi@NCA-4 aerogel, heat it with an alcohol lamp, and use a mobile phone to record the changes in the petals.
[0037] Step 5: Use CST electromagnetic field simulation software to simulate the FeNi 10 The radar stealth performance of @NCA-4 aerogel is simulated, and the calculation formula of its radar cross-section is as follows:
[0038] Step 6: The prepared FeNi@NCA-4 aerogel material is immersed in melted paraffin as a substrate to form a ring. The density of the aerogel is calculated to obtain that the material accounts for 10 wt.% of the total mass of the ring. The electromagnetic parameters of the material are measured by a vector network analyzer. According to the transmission line theory, the calculation formula for the reflection loss of the material to the electromagnetic wave is as follows: .
[0039] Figure 1 The X-ray diffraction patterns of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorbing materials provided in Examples 1, 2, 3 and 4 of the present invention show that the diffraction peaks of the four samples at 44.3°, 51.6° and 76.2° are the (111), (200) and (220) crystal planes of the FeNi alloy, among which the diffraction peak at 26.3° originates from the graphite carbon obtained by pyrolysis of COF, corresponding to the characteristic diffraction peak of the graphite (002) crystal plane, indicating that the FeNi@NCA aerogel has high purity, stable product, and is conducive to industrial production and promotion.
[0040] Figure 2 This is a scanning electron micrograph of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorber provided in Example 3 of the present invention. The COF-derived magnetic nitrogen-doped porous carbon aerogel is a porous structure composed of regular nanospheres, which are about 320 nm in size and are evenly distributed on the surface of the carbon microspheres and in the pores.
[0041] Figure 3 This is a transmission electron micrograph of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorbing material provided in Example 3 of the present invention. A large number of black cubic blocks are evenly dispersed on the gray matter stacked with spherical particles, wherein the gray spherical matter is carbon aerogel and the black cubic blocks are FeNi 10 The results show that the metal ions are thermally reduced and converted into uniformly distributed cubic FeNi nanoparticles in the aerogel pores. 10 Alloy nanoparticles.
[0042] Figure 4a to Figure 4b The nitrogen adsorption-desorption isotherms and pore size distribution of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorber provided in Examples 1, 2, 3 and 4 of the present invention, respectively. The isotherm curves of all samples show a typical IV type, indicating that micropores and mesopores coexist, which is consistent with their pore size distribution. Micro / mesopores can produce more interfaces, providing a large number of active centers for multiple reflections and absorption of electromagnetic waves.
[0043] Figure 5Vibrating sample magnetometer (VSM) graph of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorber provided in Examples 1, 2, 3 and 4 of the present invention. 10 @NCA-1, FeNi 10 @NCA-2, FeNi 10 @NCA-3 and FeNi 10 @NCA-4's saturation magnetization ( M s ) values are 32.4, 23.5, 13.7 and 8.9 emu / g respectively. M s The increase in helps to improve the magnetic loss and obtain good wave absorbing performance.
[0044] Figure 6a to Figure 6d The electromagnetic wave absorption diagram of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorbing material provided in Examples 1, 2, 3 and 4 of the present invention. Figure 6a is the electromagnetic reflection loss of the sample provided in Example 1, Figure 6b is the electromagnetic reflection loss of the sample provided in Example 2, Figure 6c is the electromagnetic reflection loss of the sample provided in Example 3, Figure 6d It is the electromagnetic reflection loss of the sample provided in Example 4. When the filling ratio is 10%, FeNi 10 @NCA-1, FeNi 10 @NCA-2 and FeNi 10 @NCA-4 RL min can reach −22.1 dB, −57.9 dB and −55.1 dB respectively, and the matching thicknesses are 2.10 mm, 3.30 mm and 4.11 mm respectively. It can be seen that FeNi 10 @NCA-3 at 17.36 GHz, RL min The matched frequency band is −63.8 dB with a matched thickness of only 2.09 mm and has a maximum EAB of 6.56 GHz (11.44-18 GHz) with a thickness of 2.28 mm.
[0045] Figure 7a to Figure 7f This is a graph showing the thermal insulation test results of the COF-derived magnetic nitrogen-doped porous carbon aerogel absorbing material provided in Example 3 of the present invention. The heating platform temperature is 120°C. Figure 7a The initial temperature is 42°C. Figure 7b After ten minutes of testing, the temperature was 46°C. Figure 7c After 20 minutes of testing, the temperature was 49°C. Figure 7d After 30 minutes of testing, the temperature was 52°C. Figure 7eAfter 40 minutes of testing, the temperature was 54°C. Figure 7f After sixty minutes of testing, the temperature was 57° C. The thermal insulation test showed that the COF-derived magnetically doped porous carbon aerogel absorber had excellent thermal insulation properties.
[0046] Although the present invention is disclosed as above in terms of preferred embodiments, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.
[0047] Note: This patent is funded by the Natural Science Foundation of Jiangxi Province (No. 20232BAB212004), the China Aerospace Science Foundation (No. 2020Z056056003) and the National Natural Science Foundation of China (No. 22265021).
Claims
1. A method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material, characterized in that: The preparation method is to obtain COF hydrogel by ultrasound-assisted self-crosslinking reaction under the action of scandium trifluoromethanesulfonate catalyst, in situ immerse the metal salt solution into the COF hydrogel, and then freeze-dry and externally heat-driven to obtain a magnetic nitrogen-doped porous carbon aerogel absorbing material; the specific steps are as follows: Step 1: Add terephthalaldehyde, 1,3,5-tri(4-aminophenyl)benzene and scandium trifluoromethanesulfonate to N,N-dimethylformamide, and after ultrasound-assisted self-crosslinking reaction, stand and crystallize to form COF gel, and then use N,N-dimethylformamide, acetone, ethanol, methanol and water to exchange solvents in sequence to obtain COF hydrogel; Step 2: Add nickel (II) chloride hexahydrate and iron (III) chloride hexahydrate solution to the COF hydrogel to allow the metal ions to be in situ immersed in the hydrogel, followed by freeze drying overnight to obtain FeNi 10 @COF aerogel; Step 3: calcining and pyrolyzing the COF aerogel under a protective gas atmosphere to obtain FeNi 10 @NCA aerogel, that is, magnetic nitrogen-doped porous carbon aerogel absorbing material.
2. The method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material according to claim 1, characterized in that: In the step 1, the ratio of terephthalaldehyde, 1,3,5-tris(4-aminophenyl)benzene, scandium trifluoromethanesulfonate and N,N-dimethylformamide is 0.0134-0.0268 g: 0.0234-0.0468 g: 0.05-0.1 g: 4 mL, and the ultrasound-assisted self-crosslinking reaction time is 5-10 minutes.
3. The method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material according to claim 1, characterized in that: In the step 2, the ratio of nickel (II) chloride hexahydrate to iron (III) chloride hexahydrate is 0.0862-0.3457 g: 0.0098-0.0393 g.
4. The method for preparing a magnetic nitrogen-doped porous carbon aerogel absorbing material according to claim 1, characterized in that: In the step 3, the protective gas is nitrogen or argon, the calcination and pyrolysis temperature is 600-900°C, the temperature is kept for 2-3 hours, and the heating rate is 2-3°C / min.
Citation Information
Patent Citations
Method for directly synthesizing single-component covalent organic framework aerogel
CN115260512A
Polyimide bead material and manufacturing method thereof
CN115768722A
Cobalt-loaded Nb2CTx / carbon aerogel as well as preparation method and application thereof
CN116099463A
Composite aerogel material as well as preparation method and application thereof
CN116726816A
Composite conductive network wave-absorbing material and preparation method thereof
CN117222213A
Cited By
Broadband wave-absorbing metamaterial with robust topological gradient structure
CN119786987A