Small-grain and low-silica-alumina-ratio lithium molecular sieve synthesized by gel seed crystal method, and preparation method and application of small-grain and low-silica-alumina-ratio lithium molecular sieve
The gel seeding method is used to synthesize small-grain, low-silicon-aluminum-ratio lithium molecular sieves, which solves the problem of insufficient adsorption performance of lithium molecular sieves, achieves efficient nitrogen adsorption and oxygen separation, and improves separation efficiency and environmental protection.
Patent Information
- Application Number
- CN202410819329.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-11
AI Technical Summary
In existing air separation technology, the adsorption performance of lithium molecular sieves is limited by the grain size and silicon-to-aluminum ratio, resulting in insufficient nitrogen adsorption capacity and insufficient separation efficiency.
The gel seed method is used to synthesize lithium molecular sieves with small grains and low silicon-to-aluminum ratio. By accurately controlling the amount of reactants and low-temperature aging, the crystallization time is shortened, the silicon-to-aluminum ratio of the molecular sieve is optimized, and its nitrogen adsorption capacity and ion exchange efficiency are improved. .
The N2 adsorption capacity and nitrogen and oxygen separation coefficient of the lithium molecular sieve are significantly improved, achieving efficient nitrogen adsorption and oxygen separation, and the process is simple, environmentally friendly and pollution-free.
Smart Images

Figure CN118754147A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adsorption materials for oxygen production, and in particular to a lithium molecular sieve with small crystal grains and low silicon-aluminum ratio, and a preparation method and application thereof. Background Art
[0002] Air is the gas surrounding the earth, covering the surface of the earth in layers, transparent, colorless and odorless. It is mainly composed of nitrogen and oxygen, and has an important impact on human survival and production. At present, air separation technologies mainly include: cryogenic air separation, membrane separation, and pressure swing adsorption (PSA).
[0003] Cryogenic air separation is an air separation method based on the principles of gas liquefaction and fractionation. Its main advantage is that it can continuously provide a large amount of high-purity gas, but the main limitations of this technology are its high construction and operating costs, high energy consumption, and the need for complex equipment. Membrane separation technology separates different gas molecules by using semipermeable membranes. The advantages of membrane separation technology are its simple equipment requirements, low energy consumption, and easy maintenance. However, the challenges of this method lie in the selectivity and durability of the membrane. Pressure swing adsorption technology separates specific gases from the air through the principle of physical adsorption. This process usually uses molecular sieves or other adsorbents to alternately adsorb and desorb gases at different pressures. Its main advantages include lower operating costs, smaller equipment footprint, and flexibility in operating conditions. However, the life and performance of the adsorbent are also important factors that restrict the further development of PSA technology.
[0004] As an adsorbent with the most ideal adsorption effect, lithium molecular sieve has a large nitrogen-oxygen separation coefficient and nitrogen adsorption capacity. Lithium molecular sieve is generally prepared by ion exchange using lithium salt solution and sodium molecular sieve.
[0005] CN1448338A relates to a method for preparing small-grain X zeolite, specifically, in a method for preparing X zeolite by a directing agent method, the aging temperature of the directing agent and the gelling temperature of the zeolite precursor are reduced to obtain a small-grain zeolite with a grain size of (0.5-1) μm, which has good thermal stability, improves the diffusion rate of the adsorbate in the grains, and improves the separation efficiency.
[0006] CN114887586A relates to a method for producing a low silicon-aluminum ratio lithium molecular sieve, which specifically produces a nanometer NaK-LSX molecular sieve with a grain size of less than 0.1 μm by increasing the alkali solution content in the synthesis system, adding metal salts, etc. and lowering the crystallization temperature. The grain size of the low silicon-aluminum ratio molecular sieve is reduced by optimizing the synthesis process to obtain a nanometer NaK-LSX molecular sieve, thereby improving the molecular sieve specific surface area and pore structure, increasing the nitrogen adsorption capacity, increasing the number of exposed unit cells, and reducing the lithium ion exchange resistance.
[0007] CN101254928A relates to a method for preparing a small-grain X zeolite with a low silicon / aluminum ratio, which specifically adopts a directing agent synthesis technology, introduces sulfuric acid or a water-soluble sulfate into a water-sodium reaction system, effectively reduces the silicon-aluminum ratio of the product, and shortens the crystallization time, thereby obtaining a high-crystallinity X zeolite with a grain size of (0.2-1.2) μm and a silicon-aluminum ratio of less than 2.30.
[0008] Therefore, further improving the adsorption performance of lithium molecular sieves is closely related to their grain size and silicon-aluminum ratio. Summary of the invention
[0009] The purpose of the present invention is to overcome the above technical shortcomings and provide a method for preparing a small-grained lithium molecular sieve with a low silicon-aluminum ratio by a gel seed method. The method can obtain a small-grained lithium molecular sieve with a low silicon-aluminum ratio. 2 The adsorption capacity is ≥32ml / g, which significantly improves the ion exchange efficiency and nitrogen adsorption capacity and can be used for oxygen production by adsorption.
[0010] To this end, the technical solution of the present invention is as follows: A preparation method for synthesizing a small-grained low silicon-aluminum ratio lithium molecular sieve by a gel seed method, comprising the following steps:
[0011] S1, feeding: the raw materials include silicon source, aluminum source, sodium source, potassium source, water and gel seed crystals, among which the silicon source is SiO 2 Aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials are based on SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=(1.95~2.05):1:(4.8~6):(1.8~2.3):(130~140) in molar ratio, wherein water is used as solvent, sodium source, potassium source and aluminum source are added in sequence and stirred until completely dissolved, after stirring and cooling, silicon source and gel seed are added; the amount of gel seed added is 0.03~0.12% of the total weight of the mixture;
[0012] S2, aging: Stir at room temperature for 2 hours, then stop stirring and let it stand for 5 to 6 hours;
[0013] S3, crystallization: start stirring, raise the temperature to 40-60°C, then stop stirring, and let it stand at a constant temperature for 6-8h; start stirring again, raise the temperature to 80-100°C, then stop stirring, and let it stand at a constant temperature for 4-6h;
[0014] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 7 to 9;
[0015] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0016] S6, crushing: crushing by mechanical crusher to a particle size of ≤5μm, and then crushing by air flow crusher to a particle size of ≤0.5μm;
[0017] S7, prepare a lithium-containing standard solution, wherein the lithium ion concentration is 2.0-2.5 mol / L and the pH is adjusted to 9-10;
[0018] S8, take the crushed material from S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeating the lithium exchange 3 to 5 times;
[0019] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve.
[0020] Furthermore, the gel seed crystals are prepared by the following steps:
[0021] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 The molar ratio of O=(16-17):1:(12-18):(3-6):(300-350) is fully mixed;
[0022] S1-2, aging: aging at a temperature of 0 to 10°C for 24 to 30 hours;
[0023] S1-3, drying: drying the aged gel at 100-120°C, with a moisture content of ≤2wt%;
[0024] S1-4, crushing: crushing by mechanical crusher to a particle size of ≤5μm, and then crushing by air flow crusher to a particle size of ≤0.5μm; to obtain gel seed crystals.
[0025] Furthermore, the silicon source includes at least one of silicon powder, silica gel, silica sol and water glass; the aluminum source includes at least one of sodium aluminate, aluminum oxide and aluminum hydroxide; the sodium source and potassium source are solid sodium hydroxide and potassium hydroxide, and the lithium-containing standard solution is at least one of lithium sulfate, lithium carbonate, lithium hydroxide and lithium chloride, preferably a mixture of lithium sulfate and lithium hydroxide, and the pH is adjusted to 9-10 by adding lithium hydroxide.
[0026] According to the method of the present invention, a small-grain lithium molecular sieve with a low silicon-aluminum ratio is prepared by a gel seed method and is used as an adsorbent in the field of oxygen production.
[0027] The present invention firstly precisely controls the amount of each reactant in the sodium-potassium system, ages at low temperature, and obtains nano-scale high-crystallinity gel seed crystals, which provide crystal nuclei and induction for the next molecular sieve crystallization process, shortening the crystallization time; and controls the molecular sieve silicon-aluminum ratio, prompting silicon and aluminum to enter the molecular sieve framework, and finally improving the molecular sieve grains and silicon-aluminum ratio. Compared with the prior art, the present invention has the following beneficial effects:
[0028] 1. Small crystal grains and low silicon-aluminum ratio molecular sieve powder grains ≤ 1μm, silicon-aluminum ratio = 2.0, used as adsorbent in the field of oxygen production, can significantly improve the nitrogen adsorption capacity, N 2 Adsorption capacity>32ml / g, nitrogen and oxygen separation coefficient≥6.28, static water adsorption rate>32%.
[0029] 2. The preparation method of the present invention does not require the designation of specific silicon sources and aluminum sources. The common silicon sources and aluminum sources can be used to prepare the molecular sieve without adding a template agent. The process is simple and the process is environmentally friendly and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a SEM image of a small-grain low-silicon molecular sieve, where the grains are ≤1μm. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0032] Embodiment 1:
[0033] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0034] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=1.95:1:4.8:1.8:130 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; wherein the silicon source is silicon powder, the aluminum source is sodium aluminate, the sodium source is sodium hydroxide, and the potassium source is potassium hydroxide;
[0035] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0036] S3, crystallization: start stirring, raise the temperature to 40°C, stop stirring, and keep it at a constant temperature for 6 hours; start stirring again, raise the temperature to 80°C, stop stirring, and keep it at a constant temperature for 4 hours;
[0037] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 7;
[0038] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0039] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0040] S7, prepare a lithium-containing standard solution, wherein the lithium ion concentration is 2.0 mol / L; the lithium-containing standard solution is prepared from lithium sulfate and lithium hydroxide, and the lithium hydroxide is used to adjust the pH to 9.
[0041] S8, take the crushed material of S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeat the lithium exchange 3 times;
[0042] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0043] The gel seed crystals in step S1 are prepared by the following steps:
[0044] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O3 :Na 2 O:K 2 O:H 2 O=16:1:12:3:300 molar ratio is fully mixed, wherein the silicon source is silicon powder, the aluminum source is sodium aluminate, the sodium source is sodium hydroxide, and the potassium source is potassium hydroxide;
[0045] S1-2, aging: aging at 0°C for 24h;
[0046] S1-3, drying: drying the aged gel at 100°C, with a moisture content of ≤2%;
[0047] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0048] Embodiment 2:
[0049] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0050] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=2.05:1:6:2.3:140 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; silicon source is silica sol, aluminum source is aluminum hydroxide, sodium source and potassium source are solid sodium hydroxide and potassium hydroxide;
[0051] S2, aging: stirring at room temperature for 2 h, then stopping stirring and letting it stand for 6 h;
[0052] S3, crystallization: start stirring, raise the temperature to 60°C, stop stirring, and keep it at a constant temperature for 8 hours; start stirring again, raise the temperature to 100°C, stop stirring, and keep it at a constant temperature for 6 hours;
[0053] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 9;
[0054] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3%;
[0055] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0056] S7, preparing a lithium-containing standard solution, wherein the lithium ion concentration is 2.5 mol / L and the pH is adjusted to 10. The lithium-containing standard solution is prepared by adding lithium hydroxide to water, and the pH is adjusted to 10 by dropping hydrochloric acid;
[0057] S8, take the crushed material of S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeat the lithium exchange 5 times;
[0058] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0059] The gel seed crystals in step S1 are prepared by the following steps:
[0060] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=17:1:18:6:350 molar ratio is fully mixed, the silicon source is silica sol, the aluminum source is aluminum hydroxide, and the sodium source and potassium source are solid sodium hydroxide and potassium hydroxide;
[0061] S1-2, aging: aging at 10°C for 30h;
[0062] S1-3, drying: drying the aged gel at 120°C, with a moisture content of ≤2%;
[0063] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0064] Embodiment 3:
[0065] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0066] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=2:1:5.4:2.05:135 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; the silicon source is silica gel, the aluminum source is alumina, and the sodium source and potassium source are the same as those in Example 1;
[0067] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0068] S3, crystallization: start stirring, heat to 50°C, stop stirring, and keep at constant temperature for 6 hours; start stirring again, heat to 90°C, stop stirring, and keep at constant temperature for 4 hours;
[0069] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 8;
[0070] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3%;
[0071] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0072] S7, preparing a lithium-containing standard solution, wherein the lithium ion concentration is 2.1 mol / L and the pH is adjusted to 9-10; the lithium-containing standard solution is prepared from lithium carbonate;
[0073] S8, take the crushed material of S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeat the lithium exchange 5 times;
[0074] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0075] The gel seed crystals in step S1 are prepared by the following steps:
[0076] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O3 :Na 2 O:K 2 O:H 2 O=16.5:1:15:4.5:325 molar ratio is fully mixed, wherein the silicon source is silica gel, the aluminum source is alumina, and the sodium source and potassium source are the same as those in Example 1;
[0077] S1-2, aging: aging at 5°C for 24h;
[0078] S1-3, drying: drying the aged gel at 110°C, with a moisture content of ≤2%;
[0079] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0080] Embodiment 4:
[0081] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0082] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=2:1:5.4:2.05:135 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; silicon source, aluminum source, sodium source and potassium source are the same as those in Example 1;
[0083] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0084] S3, crystallization: start stirring, heat to 50°C, stop stirring, and keep at constant temperature for 6 hours; start stirring again, heat to 90°C, stop stirring, and keep at constant temperature for 4 hours;
[0085] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 8;
[0086] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0087] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0088] S7, prepare a lithium-containing standard solution, the lithium ion concentration is 2.2 mol / L and the pH is adjusted to 9-10;
[0089] S8, take the crushed material from S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeating the lithium exchange 3 to 5 times;
[0090] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0091] The gel seed crystals in step S1 are prepared by the following steps:
[0092] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=16.5:1:15:4.5:325 molar ratio is fully mixed, and the silicon source, aluminum source, sodium source and potassium source are the same as in Example 1;
[0093] S1-2, aging: aging at 5°C for 24h;
[0094] S1-3, drying: drying the aged gel at 110°C, with a moisture content of ≤2wt%;
[0095] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0096] Embodiment 5:
[0097] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0098] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=2:1:5.4:2.05:135 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; silicon source, aluminum source, sodium source and potassium source are the same as those in Example 1;
[0099] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0100] S3, crystallization: start stirring, heat to 50°C, stop stirring, and keep at constant temperature for 6 hours; start stirring again, heat to 90°C, stop stirring, and keep at constant temperature for 4 hours;
[0101] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 8;
[0102] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0103] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0104] S7, prepare a lithium-containing standard solution, the lithium ion concentration is 2.3 mol / L and the pH is adjusted to 9-10;
[0105] S8, take the crushed material of S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeat the lithium exchange 4 times;
[0106] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0107] The gel seed crystals in step S1 are prepared by the following steps:
[0108] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2O=16.5:1:15:4.5:325 molar ratio is fully mixed, and the silicon source, aluminum source, sodium source and potassium source are the same as in Example 1;
[0109] S1-2, aging: aging at 5°C for 24h;
[0110] S1-3, drying: drying the aged gel at 110°C, with a moisture content of ≤2wt%;
[0111] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0112] Embodiment 6:
[0113] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0114] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=2:1:5.4:2.05:135 molar ratio, add sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stir and cool, add silicon source and gel seed; silicon source, aluminum source, sodium source and potassium source are the same as those in Example 1;
[0115] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0116] S3, crystallization: start stirring, heat to 50°C, stop stirring, and keep at constant temperature for 6 hours; start stirring again, heat to 90°C, stop stirring, and keep at constant temperature for 4 hours;
[0117] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 8;
[0118] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0119] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0120] S7, prepare a lithium-containing standard solution, the lithium ion concentration is 2.4 mol / L and the pH is adjusted to 9-10;
[0121] S8, take the crushed material from S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeating the lithium exchange 3 to 5 times;
[0122] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0123] The gel seed crystals in step S1 are prepared by the following steps:
[0124] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2 O=16.5:1:15:4.5:325 molar ratio is fully mixed, and the silicon source, aluminum source, sodium source and potassium source are the same as in Example 1;
[0125] S1-2, aging: aging at 5°C for 24h;
[0126] S1-3, drying: drying the aged gel at 110°C, with a moisture content of ≤2wt%;
[0127] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0128] Embodiment 7:
[0129] A preparation method of a small-grain, low-silicon-to-aluminum ratio lithium molecular sieve synthesized by a gel seed method comprises the following steps:
[0130] S1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the raw materials in the synthesis system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2O:H 2 O=2:1:5.4:2.05:135 molar ratio, adding sodium source, potassium source and aluminum source in pure water solvent in sequence while stirring until completely dissolved, stirring and cooling, adding silicon source and gel seed; wherein the silicon source is water glass, the aluminum source is aluminum hydroxide, and the sodium source and potassium source are solid sodium hydroxide and potassium hydroxide;
[0131] S2, aging: stirring at room temperature for 2 hours, then stopping stirring and letting it stand for 5 hours;
[0132] S3, crystallization: start stirring, heat to 50°C, stop stirring, and keep at constant temperature for 6 hours; start stirring again, heat to 90°C, stop stirring, and keep at constant temperature for 4 hours;
[0133] S4, washing: centrifugally washing the crystallized material in a centrifuge until the pH value is 8;
[0134] S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%;
[0135] S6, crushing: mechanical crushing, the particle size should be ≤5μm, and then crushed by air flow mill, the particle size should be ≤0.5μm;
[0136] S7, prepare a lithium-containing standard solution with lithium chloride, wherein the lithium ion concentration is 2.5 mol / L and the pH is adjusted to 9-10;
[0137] S8, take the crushed material from S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeating the lithium exchange 3 to 5 times;
[0138] S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve;
[0139] The gel seed crystals in step S1 are prepared by the following steps:
[0140] S1-1, feeding: silicon source is SiO 2 The aluminum source is Al 2 O 3 Sodium source is Na 2 O, potassium source is K 2 O, the reaction raw materials in the system are calculated according to SiO 2 :Al 2 O 3 :Na 2 O:K 2 O:H 2The molar ratio of O=16.5:1:15:4.5:325 is fully mixed, wherein the silicon source is water glass, the aluminum source is aluminum hydroxide, and the sodium source and potassium source are solid sodium hydroxide and potassium hydroxide;
[0141] S1-2, aging: aging at 5°C for 24h;
[0142] S1-3, drying: drying the aged gel at 110°C, with a moisture content of ≤2wt%;
[0143] S1-4, crushing: crushing by mechanical means until the particle size is less than 5 μm, and then crushing by air flow mill until the particle size is less than 0.5 μm, thus obtaining gel seed crystals;
[0144] The small-grain low silicon-aluminum ratio molecular sieve obtained in the above embodiments 1 to 7 is exchanged with lithium to obtain a lithium molecular sieve, which is used as an oxygen or nitrogen adsorbent. The addition ratio of the gel seed crystals is 0.03 to 0.12% of the total weight of the mixture.
[0145] Lithium molecular sieves are exchanged for lithium in the following manner:
[0146] Take 10g of the above-mentioned small-grain low silicon-aluminum ratio molecular sieve sample, load it into the exchange column, and then add 500ml of lithium-containing standard solution with a lithium ion concentration of 2.0-2.5mol / L. After stirring in a 90-100℃ water bath for 2h, stop stirring, filter, and wash to obtain a filter cake. The sample is mixed with the prepared lithium-containing standard solution again, and the exchange is repeated 3-5 times to obtain lithium molecular sieves with different exchange degrees. Then ICP-AES is used to measure the lithium ion content, thereby calculating the lithium exchange degree.
[0147] The prepared lithium molecular sieve is used to produce oxygen from the air, and remove nitrogen by adsorption to separate oxygen and nitrogen. By changing the lithium ion concentration, the separation coefficient of oxygen and nitrogen and the adsorption amount of nitrogen are verified. The experimental data are listed in the following table:
[0148]
[0149] The data in the table above show that the concentration of lithium-containing standard solution used for lithium exchange is 2.0-2.5 mol / L, the lithium exchange degree is high, N 2 The adsorption capacity is >32ml / g, the nitrogen-oxygen separation coefficient is ≥6.28, and the static water adsorption rate is >32%. Ion exchange is a dynamic reversible process. If the lithium concentration is too low, the exchange is not complete. If the lithium concentration is too high, the lithium ions will be converted in a reversible direction. Therefore, the lithium ion concentration in the lithium-containing standard solution used for lithium exchange is 2.0-2.5mol / L.
[0150] The gel seed crystals obtained in Example 1 above were used to synthesize small-grained Si-Al molecular sieves by changing the addition ratio of the gel seed crystals to obtain the following table:
[0151]
[0152] The data in the above table show that the addition ratio of the gel seed crystals is 0.03-0.12% of the total weight of the mixture, which is a preferred solution, with a relative crystallinity of >100, a silicon-aluminum ratio of 2.0, and a D50 particle size of ≤1 μm.
[0153] The present invention is not limited to the above-mentioned embodiments. On the basis of the technical solution disclosed in the present invention, technicians in this field can make some substitutions and deformations to some technical features therein according to the disclosed technical content without creative labor, and these substitutions and deformations are all within the protection scope of the present invention.
Claims
1. A method for preparing a small-grain, low-silicon-aluminum ratio lithium molecular sieve synthesized by a gel seed method, characterized in that: The following steps are involved: S1, feeding: the raw materials include silicon source, aluminum source, sodium source, potassium source, water and gel seed crystals, wherein the silicon source is calculated as SiO2, the aluminum source is calculated as Al2O3, the sodium source is calculated as Na2O, and the potassium source is calculated as K2O. The raw materials are composed of the molar ratio of SiO2:Al2O3:Na2O:K2O:H2O=(1.95-2.05):1:(4.8-6):(1.8-2.3):(130-140), wherein water is used as a solvent, and the sodium source, potassium source and aluminum source are added in sequence and stirred until completely dissolved. After stirring and cooling, the silicon source and gel seed crystals are added; the amount of gel seed crystals added is 0.03-0.12% of the total weight of the mixture; S2, aging: Stir at room temperature for 2 hours, then stop stirring and let it stand for 5 to 6 hours; S3, crystallization: start stirring, raise the temperature to 40-60°C, then stop stirring, and let it stand at a constant temperature for 6-8h; start stirring again, raise the temperature to 80-100°C, then stop stirring, and let it stand at a constant temperature for 4-6h; S4, washing: centrifuge the crystallized material in a centrifuge to wash it until the pH value is 7-9; S5, drying: flash drying the washed material in a flash evaporator, with the moisture content ≤ 0.3wt%; S6, crushing: crushing by mechanical crusher to a particle size of ≤5μm, and then crushing by air flow crusher to a particle size of ≤0.5μm; S7, prepare a lithium-containing standard solution, the lithium ion concentration is 2.0-2.5 mol / L and the pH is adjusted to 9-10; S8, take the crushed material from S6 and load it into the exchange column, add the lithium-containing standard solution prepared in S7 into the exchange column to perform lithium exchange for 2 hours, take out the crushed material, filter it, and then load it into the exchange column, repeating the lithium exchange 3 to 5 times; S9, drying and crushing the molecular sieve after lithium exchange to obtain a lithium molecular sieve.
2. The method for preparing a small-grained low silicon-aluminum ratio lithium molecular sieve synthesized by a gel seed method according to claim 1, characterized in that: The gel seed crystals are prepared by the following steps: S1-1, feeding: silicon source is calculated as SiO2, aluminum source is calculated as Al2O3, sodium source is calculated as Na2O, potassium source is calculated as K2O, and they are fully mixed according to the molar ratio of SiO2:Al2O3:Na2O:K2O:H2O=(16-17):1:(12-18):(3-6):(300-350); S1-2, aging: aging at a temperature of 0 to 10°C for 24 to 30 hours; S1-3, drying: drying the aged gel at 100-120°C, with a moisture content of ≤2wt%; S1-4, crushing: crushing by mechanical crusher to a particle size of ≤5μm, and then crushing by air flow crusher to a particle size of ≤0.5μm; to obtain gel seed crystals.
3. The method for preparing a small-grained low silicon-aluminum ratio lithium molecular sieve synthesized by a gel seed method according to claim 1 or 2, characterized in that: The silicon source includes at least one of silicon powder, silica gel, silica sol and water glass; the aluminum source includes at least one of sodium aluminate, aluminum oxide and aluminum hydroxide; the sodium source and potassium source are solid sodium hydroxide and potassium hydroxide, and the lithium-containing standard solution is prepared from at least one of lithium sulfate, lithium carbonate, lithium hydroxide and lithium chloride.
4. The method for preparing a small-grained low silicon-aluminum ratio lithium molecular sieve synthesized by a gel seed method according to claim 3, characterized in that: The lithium-containing standard solution is a mixture of lithium sulfate and lithium hydroxide, and the pH value is adjusted to 9-10 by lithium hydroxide.
5. A gel seed method for synthesizing a small-grain, low-silicon-aluminum ratio lithium molecular sieve, characterized in that: Prepared according to the method of any one of claims 1 to 4.
6. The use of a gel seed method for synthesizing a small-grained lithium molecular sieve with a low silicon-aluminum ratio according to claim 5, characterized in that: Used as adsorbent in the field of oxygen production.
Citation Information
Patent Citations
Method for preparing fine-grain low silica alumina ratio X zeolite
CN101254928A
Production method of lithium molecular sieve with low silica-alumina ratio
CN114887586A
Process for preparing fine-grain X zeolite
CN1448338A
Preparation method of lithium type low-silica-alumina ratio molecular sieve
CN108675314A
Preparation method and application of small-grain low-silicon X-type molecular sieve
CN114988427A
Cited By
Efficient oxygen production molecular sieve and continuous production process and application thereof