High-density alumina aerogel and preparation method thereof
Through the four-step preparation method of organic aluminum source and chelating agent, the problem of insufficient density and thermal conductivity of alumina aerogel is solved, and an alumina aerogel with high density, high strength and low thermal conductivity is prepared, which is suitable for high temperature insulation. Thermal pads to meet the needs of aerospace and other fields.
Patent Information
- Application Number
- CN202410960920.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult to prepare alumina aerogels with high density and low thermal conductivity using existing technology. In traditional methods, alumina sol has low density and insufficient elastic modulus, making it unable to meet the requirements of high-temperature thermal insulation pads.
Using organic aluminum sources and chelating agents as precursors, alumina aerogels with high density, high strength and low thermal conductivity are prepared through a four-step method of alumina sol preparation, aging, supercritical strengthening and drying, and heat treatment.
The prepared alumina aerogel has the characteristics of high elastic modulus, high temperature resistance of 1200°C, and low thermal conductivity. The compressive elastic modulus reaches 24-241MPa, and the thermal conductivity at room temperature is 0.028-0.043W/(m·K). It is suitable for High temperature insulation material.
Smart Images

Figure CN118754177A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of aerogel materials, and particularly relates to a high-density alumina aerogel and a preparation method thereof. Background Art
[0002] Fasteners are one of the key structures in the aerospace field. One common form is high-temperature resistant structural parts-insulation pads-conventional structural parts, which are fastened by nuts with a certain torque. Insulation pads should have high pressure-bearing performance (small deformation under compression load), while taking into account good temperature resistance (above 1000℃) and thermal insulation performance. The typical requirements are that the compression elastic modulus reaches more than 100MPa and the thermal conductivity is less than 0.05W / (m·K). Traditional insulation materials cannot meet the above requirements at the same time.
[0003] Alumina aerogel is a high-temperature resistant nanoporous material with extremely low thermal conductivity. It has broad application prospects as a high-temperature thermal insulation material. However, the alumina aerogel prepared by conventional methods has a low density, and the elastic modulus is usually below 10MPa. Increasing the density is an effective method to improve the mechanical properties of aerogels, but the current method of using organic aluminum sources or inorganic aluminum sources to prepare alumina aerogels based on the sol-gel method cannot produce high-density alumina aerogels because the solid content of the alumina sol is difficult to increase. Organic aluminum sources have high reactivity. When they are used as precursors to prepare high-solid-content alumina sols, violent reactions and rapid gelation are very likely to occur, making it difficult to form a stable sol, so high-density alumina aerogels cannot be obtained. The inorganic aluminum source (such as aluminum chloride and aluminum nitrate) itself has a low alumina content, so its sol solid content cannot be significantly increased, so it is also difficult to obtain high-density alumina aerogels, and a cumbersome solvent replacement process is required.
[0004] Therefore, the preparation of high-density, high-strength alumina aerogels with low thermal conductivity remains a major challenge. Summary of the invention
[0005] In view of the problem that high-density, low-thermal conductivity alumina aerogel cannot be prepared in the prior art, the present invention provides a high-density alumina aerogel and a preparation method thereof. The prepared alumina aerogel material has the characteristics of high elastic modulus, high temperature resistance of 1200°C, and low thermal conductivity. As a new type of rigid insulation pad material, it has broad application prospects.
[0006] The present invention intends to use an organic aluminum source as a precursor and a chelating agent as a capping substance to prepare alumina aerogel with high density, high strength, high temperature resistance and low thermal conductivity.
[0007] The preparation method of the invention comprises four steps: preparation of alumina sol; aging; supercritical strengthening and drying; and heat treatment.
[0008] The purpose of the present invention is achieved through the following technical solutions:
[0009] A method for preparing high-density alumina aerogel comprises the following steps:
[0010] 1) Preparation of alumina sol: Mix the chelating agent and the alcohol substance I, and stir evenly to obtain a chelating agent solution;
[0011] Slowly add the organic aluminum source to the chelating agent solution and mix evenly, and react for 1-24 hours to obtain an aluminum source precursor solution;
[0012] Add the silicon source precursor to the aluminum source precursor solution, stir evenly, then slowly add the alcohol substance II and water, and react for 1-24 hours to obtain an aluminum oxide sol;
[0013] The molar ratio of the chelating agent, alcohol substance I, silicon source precursor, water, alcohol substance II, and organic aluminum source is (0.30-1.2):(0.5-6):(0.1-1):(1.8-3.5):(0.5-4):1;
[0014] The chelating agent is selected from ethyl acetoacetate or acetylacetone;
[0015] The alcohol substance is selected from any one of ethanol, n-propanol, isopropanol, n-butanol, sec-butanol and tert-butanol;
[0016] The organic aluminum source is selected from aluminum ethoxide or aluminum sec-butoxide;
[0017] The silicon source precursor is selected from any one of methyl orthosilicate, ethyl orthosilicate, polyethyl orthosilicate, propyl orthosilicate, and isopropyl orthosilicate;
[0018] 2) Aging treatment: The alumina sol is placed at 40-120°C for 2-48 hours to age it and obtain an alumina gel;
[0019] 3) Supercritical strengthening and drying: Using alcohol as the drying medium, the alumina gel and the alcohol are placed in an autoclave, heated together to above the critical point of the alcohol for 8-48 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0020] The volume ratio of alcohol substance to alumina gel is (0.50-2.0):1;
[0021] The alcohol substance is selected from any one of ethanol, n-propanol, isopropanol, n-butanol, sec-butanol and tert-butanol.
[0022] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 700-1100°C for 2-24 hours, and then cooled naturally to obtain a high-density alumina aerogel. The high-density alumina aerogel has the following typical technical indicators:
[0023] (1) Typical density is 0.09-0.26g / cm 3 , the compression elastic modulus reaches 24-241MPa, and the compression stress of 3% deformation reaches 0.5-4.2MPa;
[0024] (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 97-123m 2 / g;
[0025] (3) The typical value of thermal conductivity at room temperature is 0.028-0.043 W / (m·K).
[0026] Furthermore, in step 1), the chelating agent is selected from ethyl acetoacetate.
[0027] Furthermore, in step 1) and step 3), the alcohol substance is selected from ethanol.
[0028] The present invention also relates to a high-density alumina aerogel, which is obtained by using the above-mentioned method for preparing a high-density alumina aerogel. The high-density alumina aerogel has the following typical technical indicators:
[0029] (1) Typical density is 0.09-0.26g / cm 3 , the compression elastic modulus reaches 24-241MPa, and the compression stress of 3% deformation reaches 0.5-4.2MPa;
[0030] (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 97-123m 2 / g;
[0031] (3) The typical value of thermal conductivity at room temperature is 0.028-0.043 W / (m·K).
[0032] Compared with the prior art, the present invention has the following advantages:
[0033] 1. The method for preparing a high-density alumina aerogel described in the present invention replaces part of the alcohol solvent with a chelating agent during the preparation of the alumina sol. On the one hand, the chelating agent reacts with the organic aluminum source to form an appropriate end-capping reaction, the reaction activity is reduced, and the reaction rate is effectively controlled; on the other hand, the proportion of the alcohol solvent is reduced, so that a stable and uniform high-solid content alumina sol can be prepared, and at the same time, the introduction of an organic silicon source further increases the cross-linking degree of the alumina gel, thereby obtaining a high-density and high-strength alumina aerogel. Since the reaction is well controlled, the alumina aerogel has a uniform particle size and nanopore size, and there are almost no macropores, which ensures that the thermal conductivity of the high-density aerogel is still low.
[0034] 2. The method for preparing a high-density alumina aerogel described in the present invention maintains the high-density alumina gel under high temperature and high pressure conditions for a long time. The alcohol solvent in the supercritical state can significantly increase the activity of the unreacted aluminum source groups in the alumina gel, allowing them to break through the end-capping effect of the chelating agent and further undergo hydrolysis and condensation reactions with the water in the gel, so that the network structure is fully cross-linked, thereby significantly enhancing it.
[0035] 3. In the method for preparing a high-density alumina aerogel described in the present invention, the added organic silicon source is converted into a silicon oxide component and enters the network structure of the alumina aerogel, which can further enhance and significantly inhibit the sintering and phase transition of the alumina aerogel at high temperatures, thereby preparing a high-density alumina aerogel with good strength and temperature resistance.
[0036] 4. The raw materials described in the present invention are easily available, and a high-solid-content alumina sol and a high-density alumina aerogel can be prepared by a simple process, avoiding the cumbersome processes such as solvent replacement and liquid phase modification in conventional methods, and the preparation process is stable and controllable. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 is a physical photograph of the high-density alumina aerogel prepared in Example 2 of the present invention;
[0038] Figure 2 is a scanning electron microscope photograph of the high-density alumina aerogel prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0039] The present invention is further described in detail below by way of examples, but these examples should not be considered as limiting the present invention.
[0040] Embodiment 1:
[0041] A method for preparing high-density alumina aerogel comprises the following steps:
[0042] 1) Preparation of alumina sol: ethyl acetoacetate and ethanol I are mixed and stirred to obtain ethyl acetoacetate solution;
[0043] Slowly add aluminum ethoxide to the ethyl acetoacetate solution and mix well. After reacting for 2 hours, an aluminum ethoxide solution is obtained.
[0044] Methyl orthosilyl ester is added to the ethanol aluminum solution and stirred evenly, and then a mixed solution of ethanol II and water is slowly added thereto, and after reacting for 2 hours, an alumina sol is obtained;
[0045] The molar ratio of ethyl acetoacetate, ethanol I, methyl orthosilicate, water, ethanol II, and aluminum ethoxide is 0.60:2.0:0.40:2.0:0.5:1;
[0046] 2) Aging treatment: The alumina sol is placed at 100°C for 10 hours to age it and obtain an alumina gel;
[0047] 3) Supercritical strengthening and drying: Using ethanol as the drying medium, the alumina gel and ethanol are placed in an autoclave, heated together to above the critical point of ethanol and maintained for 14 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0048] The volume ratio of ethanol to alumina gel is 0.8:1;
[0049] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 1000°C for 10 hours, and then cooled naturally to obtain a high-density alumina aerogel.
[0050] The obtained high-density alumina aerogel has the following properties:
[0051] (1) Density: 0.19 g / cm 3 , the compression elastic modulus is 116MPa, and the compression strength at 3% deformation is 2.6MPa;
[0052] (2) After heat treatment at 1200℃ in a muffle furnace for 2h, the specific surface area is 123m 2 / g;
[0053] (3) The typical value of thermal conductivity at room temperature is 0.036 W / (m·K).
[0054] Embodiment 2:
[0055] A method for preparing high-density alumina aerogel comprises the following steps:
[0056] 1) Preparation of alumina sol: ethyl acetoacetate and ethanol I are mixed and stirred to obtain ethyl acetoacetate solution;
[0057] Slowly add aluminum ethoxide to the ethyl acetoacetate solution and mix well. After reacting for 1 hour, an aluminum ethoxide solution is obtained.
[0058] Methyl orthosilyl ester is added to the ethanol aluminum solution and stirred evenly, and then a mixed solution of ethanol II and water is slowly added thereto, and after reacting for 2 hours, an alumina sol is obtained;
[0059] The molar ratio of ethyl acetoacetate, ethanol I, methyl orthosilicate, water, ethanol II, and aluminum ethoxide is 0.30:6.0:0.1:1.8:4:1;
[0060] 2) Aging treatment: The alumina sol is placed at 40°C for 48 hours to age and obtain an alumina gel;
[0061] 3) Supercritical strengthening and drying: Using ethanol as the drying medium, the alumina gel and ethanol are placed in an autoclave, heated together to above the critical point of ethanol and maintained for 14 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0062] The volume ratio of ethanol to alumina gel is 0.8:1;
[0063] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 1100° C. for 2 h, and then cooled naturally to obtain a high-density alumina aerogel.
[0064] Figure 1 This is a real photo of the high-density alumina aerogel prepared in Example 2; the obtained high-density alumina aerogel has the following properties:
[0065] (1) Density: 0.09 g / cm 3 , the compression elastic modulus is 24MPa, and the compression strength at 3% deformation is 0.5MPa;
[0066] (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the specific surface area is 117m 2 / g;
[0067] (3) The typical value of thermal conductivity at room temperature is 0.028 W / (m·K).
[0068] Embodiment 3:
[0069] A method for preparing high-density alumina aerogel comprises the following steps:
[0070] 1) Preparation of alumina sol: ethyl acetoacetate and ethanol I are mixed and stirred to obtain ethyl acetoacetate solution;
[0071] Slowly add aluminum ethoxide to the ethyl acetoacetate solution and mix well, and react for 24 hours to obtain an aluminum ethoxide solution;
[0072] Methyl orthosilyl ester was added to the ethanol aluminum solution and stirred evenly, and then a mixed solution of ethanol II and water was slowly added thereto. After reacting for 24 hours, an alumina sol was obtained;
[0073] The molar ratio of ethyl acetoacetate, ethanol I, methyl orthosilicate, water, ethanol II, and aluminum ethoxide is 1.2:0.5:1:3.5:0.5:1;
[0074] 2) Aging treatment: The alumina sol is placed at 120°C for 2 hours to age it and obtain an alumina gel;
[0075] 3) Supercritical strengthening and drying: Using ethanol as the drying medium, the alumina gel and ethanol are placed in an autoclave, heated together to above the critical point of ethanol and maintained for 24 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0076] The volume ratio of ethanol to alumina gel is 2.0:1;
[0077] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 1100° C. for 2 h, and then cooled naturally to obtain a high-density alumina aerogel.
[0078] Figure 2 is a scanning electron microscope photograph of the high-density alumina aerogel prepared in Example 3; the obtained high-density alumina aerogel has the following properties:
[0079] (1) Density: 0.22 g / cm 3 , the compression elastic modulus reaches 192MPa, and the compression strength at 3% deformation is 3.5MPa;
[0080] (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 104m 2 / g;
[0081] (3) The typical value of thermal conductivity at room temperature is 0.040 W / (m·K).
[0082] Embodiment 4:
[0083] A method for preparing high-density alumina aerogel comprises the following steps:
[0084] 1) Preparation of alumina sol: acetylacetone and ethanol I are mixed and stirred to obtain an acetylacetone solution;
[0085] Slowly add aluminum ethoxide to the acetylacetone solution and mix well. After reacting for 2 hours, an aluminum ethoxide solution is obtained.
[0086] Add polyethyl silicate to the ethanol aluminum solution and stir evenly, then slowly add a mixed solution of ethanol II and water, and react for 2 hours to obtain an alumina sol;
[0087] The molar ratio of acetylacetone, ethanol I, polyethyl silicate, water, ethanol II, and aluminum ethanol is 1.0:0.5:0.35:2.2:0.5:1;
[0088] 2) Aging treatment: The alumina sol is placed at 100°C for 10 hours to age it and obtain an alumina gel;
[0089] 3) Supercritical strengthening and drying: Using ethanol as the drying medium, the alumina gel and ethanol are placed in an autoclave, heated together to above the critical point of ethanol and maintained for 14 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0090] The volume ratio of ethanol to alumina gel is 1:1;
[0091] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 1000°C for 10 hours, and then cooled naturally to obtain a high-density alumina aerogel.
[0092] The obtained high-density alumina aerogel has the following properties:
[0093] (1) Density: 0.26 g / cm 3 , the compression elastic modulus reaches 241MPa, and the compression strength at 3% deformation is 4.2MPa;
[0094] (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 97m 2 / g;
[0095] (3) The typical value of thermal conductivity at room temperature is 0.043 W / (m·K).
[0096] Embodiment 5:
[0097] A method for preparing high-density alumina aerogel comprises the following steps:
[0098] 1) Preparation of alumina sol: acetylacetone and isopropanol I are mixed and stirred to obtain an acetylacetone solution;
[0099] Slowly add aluminum sec-butoxide to the acetylacetone solution and mix well. After reacting for 2 hours, an aluminum sec-butoxide solution is obtained.
[0100] Add isopropyl orthosilyl ester to the aluminum sec-butoxide solution and stir evenly, then slowly add a mixed solution of isopropanol II and water, and react for 2 hours to obtain an alumina sol;
[0101] The molar ratio of acetylacetone, isopropanol I, isopropyl orthosilicate, water, isopropanol II, and aluminum sec-butoxide is 0.55:2.0:0.33:2.4:0.5:1;
[0102] 2) Aging treatment: The alumina sol is placed at 100°C for 10 hours to age it and obtain an alumina gel;
[0103] 3) Supercritical strengthening and drying: using isopropanol as the drying medium, placing the alumina gel and isopropanol in an autoclave, heating them together to above the critical point of isopropanol for 12 hours, and then releasing the pressure to completely discharge the fluid in the autoclave to obtain alumina aerogel;
[0104] The volume ratio of isopropanol to alumina gel is 0.9:1;
[0105] 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 950°C for 10 hours, and then cooled naturally to obtain a high-density alumina aerogel.
[0106] The obtained high-density alumina aerogel has the following properties:
[0107] (1) Density: 0.17 g / cm 3 , the compression elastic modulus is 104MPa, and the compression strength at 3% deformation is 2.0MPa;
[0108] (2) After heat treatment at 1200℃ in a muffle furnace for 2h, the specific surface area is 122m 2 / g;
[0109] (3) The typical value of thermal conductivity at room temperature is 0.035 W / (m·K).
[0110] Comparative Example 1:
[0111] The process for preparing alumina aerogel is different from that of Example 1, except that the molar ratio of ethyl acetoacetate to aluminum ethoxide in step 1) is 1.5:1;
[0112] The obtained alumina aerogel has a compressive elastic modulus of 74 MPa and a compressive stress of 1.6 MPa at 3% deformation.
[0113] For this patent, the higher the compressive elastic modulus and compressive stress, the better, and the lower the thermal conductivity, the better; the compressive elastic modulus and compressive stress of aerogel are greatly affected by density, and show an exponential upward trend with increasing density.
[0114] Comparison between Comparative Example 1 and Example 3 shows that Example 3 has a low density and thus a low compression modulus. Comparative Example 1 reflects the effect of an excess of a chelating agent on the compression modulus, because the density of Comparative Example 1 is not significantly reduced compared to Example 1, so the compression modulus is significantly lower than that of Example 1, but still higher than that of Example 3.
[0115] Comparative Example 1 shows that an excessive amount of chelating agent will significantly inhibit the hydrolysis and polycondensation reactions of the aluminum source precursor, weaken the integrity of the alumina aerogel network structure, and thus reduce the pressure-bearing performance of the aerogel.
[0116] Comparative Example 2:
[0117] The process for preparing alumina aerogel is different from that of Example 1, except that the molar ratio of ethanol I to aluminum ethanol in step 1) is 12:1;
[0118] The obtained alumina aerogel has a density of 0.07 g / cm 3 , the compression elastic modulus is 17MPa, and the compression strength at 3% deformation is 0.35MPa.
[0119] Comparative Example 2 shows that a high solvent ratio significantly reduces the solid content of the sol and the density of the aerogel, thereby significantly reducing the pressure-bearing performance of the aerogel.
[0120] Comparative Example 3:
[0121] The process for preparing alumina aerogel is different from that of Example 1, except that in step 1), the molar ratio of methyl orthosilicate to aluminum ethoxide is 1.5:1;
[0122] After heat treatment at 1200℃ in a muffle furnace for 2h, the obtained alumina aerogel has a specific surface area of 64m 2 / g.
[0123] Comparative Example 3 shows that a high content of silicon source precursor will significantly reduce the aluminum-silicon ratio in the aerogel, which is not conducive to the temperature resistance of the aerogel.
[0124] Comparative Example 4:
[0125] The process for preparing alumina aerogel is different from that of Example 1, except that the molar ratio of water to aluminum ethoxide in step 1) is 1.2:1;
[0126] The obtained alumina aerogel has a compressive elastic modulus of 62 MPa and a compressive stress of 1.1 MPa at 3% deformation.
[0127] Comparative Example 4 shows that low water content will significantly reduce the degree of hydrolysis and polycondensation of the aluminum source precursor, thereby weakening the integrity of the alumina aerogel network structure and adversely affecting the pressure-bearing performance of the aerogel.
[0128] The obtained high-density alumina aerogel has the following properties:
[0129] (1) Density: 0.19 g / cm 3 , the compression elastic modulus is 116MPa, and the compression strength at 3% deformation is 2.6MPa;
[0130] (2) After heat treatment at 1200℃ in a muffle furnace for 2h, the specific surface area is 123m 2 / g;
[0131] (3) The typical value of thermal conductivity at room temperature is 0.036 W / (m·K).
[0132] Comparative Example 5:
[0133] The process for preparing alumina aerogel is different from that in Example 1, in step 3), the critical point is maintained for 3 hours;
[0134] The obtained alumina aerogel has a compressive elastic modulus of 96 MPa and a compressive stress of 1.8 MPa at 3% deformation.
[0135] Comparative Example 5 shows that the supercritical strengthening time has a great influence on the pressure bearing performance of alumina aerogel.
[0136] Comparative Example 6:
[0137] The process for preparing alumina aerogel is different from that in Example 1, in that the heat treatment temperature in step 4) is 500°C;
[0138] The obtained alumina aerogel has a compressive elastic modulus of 87 MPa and a compressive stress of 1.6 MPa at 3% deformation.
[0139] Comparative Example 6 shows that heat treatment at an appropriate temperature can further improve the strength of the alumina aerogel, and too low a heat treatment temperature will reduce the strengthening effect of the process and reduce the pressure bearing performance.
[0140] The above are only preferred implementations of the present invention. The protection scope of the present invention is not limited to the above embodiments. Various process schemes that are not substantially different from the concept of the present invention are within the protection scope of the present invention.
Claims
1. A method for preparing high-density alumina aerogel, characterized in that: The following steps are involved: 1) Preparation of alumina sol: Mix the chelating agent and the alcohol substance I, and stir evenly to obtain a chelating agent solution; Slowly add the organic aluminum source to the chelating agent solution and mix evenly, and react for 1-24 hours to obtain an aluminum source precursor solution; Add the silicon source precursor to the aluminum source precursor solution, stir evenly, then slowly add the alcohol substance II and water, and react for 1-24 hours to obtain an aluminum oxide sol; The molar ratio of the chelating agent, alcohol substance I, silicon source precursor, water, alcohol substance II, and organic aluminum source is (0.30-1.2):(0.5-6):(0.1-1):(1.8-3.5):(0.5-4):1; The chelating agent is selected from ethyl acetoacetate or acetylacetone; The alcohol substance is selected from any one of ethanol, n-propanol, isopropanol, n-butanol, sec-butanol and tert-butanol; The organic aluminum source is selected from aluminum ethoxide or aluminum sec-butoxide; The silicon source precursor is selected from any one of methyl orthosilicate, ethyl orthosilicate, polyethyl orthosilicate, propyl orthosilicate, and isopropyl orthosilicate; 2) Aging treatment: The alumina sol is placed at 40-120°C for 2-48 hours to age the alumina sol to obtain an alumina gel; 3) Supercritical strengthening and drying: Using alcohol as the drying medium, the alumina gel and the alcohol are placed in an autoclave, heated together to above the critical point of the alcohol for 8-48 hours, and then the pressure is released to completely discharge the fluid in the autoclave to obtain alumina aerogel; The volume ratio of alcohol substance to alumina gel is (0.50-2.0):1; The alcohol substance is selected from any one of ethanol, n-propanol, isopropanol, n-butanol, sec-butanol and tert-butanol. 4) Heat treatment: The alumina aerogel is placed in a high temperature furnace, heated to 700-1100°C for 2-24 hours, and then cooled naturally to obtain a high-density alumina aerogel. The high-density alumina aerogel has the following typical technical indicators: (1) Typical density is 0.09-0.26g / cm 3 , the compression elastic modulus reaches 24-241MPa, and the compression stress of 3% deformation reaches 0.5-4.2MPa; (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 97-123m 2 / g; (3) The typical value of thermal conductivity at room temperature is 0.028-0.043 W / (m·K).
2. The method for preparing a high-density alumina aerogel according to claim 1, characterized in that: In step 1), the chelating agent is selected from ethyl acetoacetate.
3. The method for preparing a high-density alumina aerogel according to claim 1, characterized in that: In step 1) and step 3), the alcohol substance is selected from ethanol.
4. A high-density alumina aerogel, characterized in that: The high-density alumina aerogel is prepared by the method for preparing the high-density alumina aerogel according to any one of claims 1 to 3, and the high-density alumina aerogel has the following typical technical indicators: (1) Typical density is 0.09-0.26g / cm 3 , the compression elastic modulus reaches 24-241MPa, and the compression stress of 3% deformation reaches 0.5-4.2MPa; (2) After heat treatment at 1200℃ for 2h in a muffle furnace, the typical specific surface area is 97-123m 2 / g; (3) The typical value of thermal conductivity at room temperature is 0.028-0.043 W / (m·K).