Indium oxide catalyst for catalyzing hydrogenation of carbon dioxide to prepare methanol as well as preparation method and application of indium oxide catalyst
Through the preparation of In2O3 catalyst, the NH3·H2O co-precipitation method is used to form a small particle structure, which solves the problem of difficulty in improving the methanol selectivity of existing catalysts at low temperatures, and achieves efficient CO2 hydrogenation to methanol reaction with excellent catalytic performance. and low-cost features.
Patent Information
- Application Number
- CN202410655445.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-10-11
AI Technical Summary
Existing carbon dioxide hydrogenation to methanol catalysts are difficult to improve methanol selectivity at low temperatures, precious metal catalysts are expensive and difficult to apply, and Cu/ZnO/Al2O3 catalysts are highly competitive in reverse water gas reactions, making it difficult to improve methanol selectivity.
Using In2O3 catalyst, it is prepared by calcining indium salt and pH regulator NH3·H2O or (NH4)2CO3 at 400-800℃. The co-precipitation method of NH3·H2O is used to form a small particle structure, control the particle size and oxygen vacancies, and improve the catalyst's performance. Specific surface area and active sites.
The catalyst preparation with simple operation, mild reaction conditions and low cost is achieved, which significantly improves methanol selectivity, and the catalyst shows excellent performance in CO2 hydrogenation to methanol.
Smart Images

Figure CN118754187A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a catalyst and a CO 2 The technical field of resource utilization, in particular to an indium oxide catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol, and a preparation method and application thereof. Background Art
[0002] Excess CO 2 Emissions seriously disrupt the balance of the natural carbon cycle, leading to environmental problems such as global warming. 2 The resource utilization of hydrogen becomes crucial. Hydrogen is one of the most effective renewable energy sources, and CO2 hydrogenation is considered a feasible and promising strategy to effectively reduce CO2 concentrations and mitigate the challenge of fossil fuel depletion.
[0003] As a clean fuel and chemical raw material, methanol is highly renewable and environmentally friendly. The development and construction of CO2 hydrogenation to methanol projects have certain economic benefits and are of great significance to environmental protection and sustainable development, and have become a research hotspot for researchers. At present, the catalysts for CO2 hydrogenation to methanol mainly include copper-based metals, precious metals and metal oxides; among them, copper-based catalysts account for about 70%, Cu / ZnO / Al 2 O 3 Catalysts have been industrialized, but competition with the reverse water gas reaction has made it difficult to improve methanol selectivity, and precious metal catalysts are expensive and difficult to put into practical use. 2 Hydrogenation to methanol catalyst is an important challenge at present. Summary of the invention
[0004] The purpose of the present invention is to provide an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol in view of the deficiencies in the prior art described above, which has the advantages of simple operation, mild reaction conditions, and can also enable the catalyst to exhibit excellent methanol selectivity through the action of a pH regulator.
[0005] Another object of the present invention is to provide a method for preparing the In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol.
[0006] The third object of the present invention is to provide the application of the In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol.
[0007] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol is prepared by using indium salt as raw material, adding a pH regulator and calcining at 400-800°C.
[0008] The indium salt is preferably In(NO 3 ) 3 ·5H 2 O.
[0009] The pH adjuster is preferably NH 3 ·H 2 O or (NH 4 ) 2 CO 3 .
[0010] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol comprises the following steps: (1) mixing indium salt and deionized water in a ratio of 1:20 to 1:30 to prepare a mixed solution; (2) using a peristaltic pump to dropwise add a pH regulator into the mixed solution and adjust the pH value of the mixed solution; (3) After the addition is completed, the temperature is adjusted to 70 to 90° C. in a constant temperature water bath and stirred continuously for 1 to 5 hours to allow the pH adjuster and the aqueous solution of the indium salt to fully contact each other, and aged for 1 to 5 hours to form a precipitate; (4) centrifuging the precipitate, washing with deionized water, and drying to obtain a precursor; (5) Place the precursor in a muffle furnace, heat it to 400-800°C and calcine it in air to form In 2 O 3 catalyst.
[0011] The concentration of the pH adjuster is 0.1M to 2M.
[0012] The peristaltic pump has a drip acceleration rate of 1 to 10 ml / min -1 .
[0013] The pH value ranges from 5 to 10.
[0014] An application of an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to produce methanol in catalytic hydrogenation of carbon dioxide to produce methanol, comprising a reduction step and a catalytic step, wherein the catalytic reaction conditions of the catalytic step are: the reaction gas is CO 2 :H 2 =1:2~1:4 gas mixture, space velocity is 5000~15000ml·g -1 ·h -1 , the reaction temperature is 240-340°C, and the pressure is 2-6Mpa.
[0015] The reduction conditions of the reduction step are: a reducing gas composed of a mixture of hydrogen and argon (wherein the content of hydrogen accounts for 10%), a reduction temperature of 250-450° C., and a reduction time of 1-3 hours.
[0016] Wherein, the In2O3 catalyst should be sieved to a mesh size of 40 to 60 meshes.
[0017] The present invention uses NH 3 ·H 2 O is used as the precipitant and is prepared by co-precipitation. The preparation process makes full use of NH 3 ·H 2 O and In(NO 3 ) 3 The interaction between the two forms a small and dense particle structure, which not only helps to increase the specific surface area of the catalyst, but also effectively promotes CO 2 and H 2 adsorption and desorption process, therefore, in CO 2 In the field of hydrogenation to methanol, the catalyst exhibits higher methanol selectivity.
[0018] Compared with the prior art, the present invention has the following beneficial effects: (1) Simple operation, short time consumption, mild reaction conditions, easy control of conditions, good reproducibility, and low preparation cost; (2) NH 3 ·H 2 O can effectively regulate In as a pH regulator 2 O 3 The particle size is reduced to increase the specific surface area and the concentration of oxygen vacancies, so that the active sites can be fully exposed; (3) It has excellent methanol selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a SEM image of the In2O3 catalyst prepared in Example 1 for catalytic hydrogenation of carbon dioxide to methanol;
[0020] Figure 2 In prepared in Comparative Example 1 2 O 3 SEM image of catalyst;
[0021] Figure 3 In prepared in Comparative Example 2 2 O 3 SEM image of catalyst;
[0022] Figure 4 The XRD patterns of the samples of Example 1, Comparative Example 1 and Comparative Example 2 are shown in FIG.
[0023] Figure 5 These are the XPS graphs of the samples of Example 1, Comparative Example 1, and Comparative Example 2. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below in conjunction with the accompanying drawings and specific examples. The examples provided in the specification only cover some embodiments, not all. The methods in the examples are conventional methods unless otherwise specified, and the reagents are conventional commercially available reagents or reagents prepared according to conventional methods unless otherwise specified. Example 1
[0025] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol, the steps of which are as follows: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M pH regulator NH 3 ·H 2 O, drop by drop into the mixed solution with a peristaltic pump, and adjust the pH of the mixed solution to 9; after the addition is completed, stir continuously for 3 hours in a constant temperature water bath at 80°C, and age for 1 hour to allow the precipitation to be fully formed; the precipitate is centrifuged, washed with deionized water, and dried to obtain a precursor; the precursor is placed in a muffle furnace and heated at 3°C·min -1 The heating rate was heated from room temperature to 600 ° C, maintained for 4 hours, and after cooling to room temperature, In 2 O 3 Catalyst samples, morphology Figure 1 shown.
[0026] In 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol includes the following steps: first, In 2 O 3 The catalyst tablets were sieved into 50 mesh, and then 0.3 g of the sieved In 2 O 3 The catalyst was placed in a fixed bed reactor and reduced for 3 h at normal pressure, 350° C., and a reducing gas composed of a mixture of hydrogen and argon (wherein the content of hydrogen was 10%); after the reduction was completed, the temperature of the fixed bed reactor was naturally cooled to 240° C., and the reducing gas was switched to the reaction gas, wherein the reaction gas was CO with a volume ratio of 2 :H 2 =1:3 mixed gas, air velocity is 8000ml·g -1 ·h -1 Then the temperature was raised to 260°C and CO was carried out under 3Mpa. 2 The hydrogenation reaction was completed after 12 hours.
[0027] The 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1. Example 2
[0028] The only difference between this embodiment and embodiment 1 is that In 2 O 3 The mesh size (40 mesh) of the catalyst sample in the application of catalytic carbon dioxide hydrogenation to methanol, the evaluation conditions and the results are shown in Appendix 1. Example 3
[0029] The only difference between this embodiment and embodiment 1 is that In 2 O 3 The mesh size (60 mesh) of the catalyst sample in the application of catalytic carbon dioxide hydrogenation to methanol, the evaluation conditions and results are shown in Appendix 1.
[0030] Conclusion: Examples 1, 2, and 3 in Table 1 are the regulation of the catalyst tablet sieving mesh number. The regulation of the tablet sieving mesh number can affect the size and distribution of the catalyst particles. A lower sieving mesh number may lead to the aggregation of larger particles, while a higher sieving mesh number may produce more evenly distributed particles, which will affect the activity and selectivity of the catalyst. Example 4
[0031] The only difference between this embodiment and embodiment 1 is that In 2 O 3 The reaction temperature (240°C) of the catalyst sample in the application of catalytic carbon dioxide hydrogenation to methanol, the evaluation conditions and results are shown in Appendix 1. Example 5
[0032] The only difference between this embodiment and embodiment 1 is that In 2 O 3 The reaction temperature (280°C) of the catalyst sample in the application of catalytic carbon dioxide hydrogenation to methanol, the evaluation conditions and results are shown in Appendix 1.
[0033] Conclusion: As shown in Table 1, Examples 1, 4, and 5 are the regulation of the catalyst reaction temperature. As the reaction temperature increases, the selectivity of methanol increases first and then decreases. This phenomenon occurs mainly due to the occurrence of competitive side reactions, especially the reverse water gas reaction (RWGS). RWGS is an endothermic reaction, so high temperature conditions are more conducive to the formation of CO. Comprehensively considered, the catalyst has the best CO selectivity at a reaction temperature of 260°C. 2 Catalytic conversion activity. Example 6
[0034] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol comprises the following steps: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M NH3 ·H 2 O, drop by drop into the mixed solution with a peristaltic pump, and adjust the pH of the mixed solution to 8; after the addition is completed, stir continuously for 3 hours in a constant temperature water bath at 80°C, and age for 1 hour to allow the precipitation to be fully formed; centrifuge the precipitate, wash with deionized water, and dry to obtain a precursor; place the precursor in a muffle furnace at 3°C·min -1 The heating rate was heated from room temperature to 600 ° C, maintained for 4 hours, and after cooling to room temperature, In 2 O 3 catalyst.
[0035] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1. Example 7
[0036] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol comprises the following steps: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M NH 3 ·H 2 O, drop by drop into the mixed solution with a peristaltic pump, and adjust the pH of the mixed solution to 10; after the addition is completed, stir continuously for 3 hours in a constant temperature water bath at 80°C, and age for 1 hour to allow the precipitation to be fully formed; the precipitate is centrifuged, washed with deionized water, and dried to obtain a precursor; the precursor is placed in a muffle furnace at 3°C·min -1 The heating rate was heated from room temperature to 600 ° C, maintained for 4 hours, and after cooling to room temperature, In 2 O 3 catalyst.
[0037] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1.
[0038] Conclusion: Examples 1, 6, and 7 are about the regulation of solution pH during the preparation process. Different pH values may lead to precipitates of different morphologies and crystalline phases, thereby affecting their surface area, pore structure, lattice defects and other properties. These properties will further affect the distribution and accessibility of the surface active sites of the catalyst, thereby affecting the catalytic activity. Example 8
[0039] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol comprises the following steps: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M NH 3 ·H 2 O, drop by drop into the mixed solution with a peristaltic pump, and adjust the pH of the mixed solution to 9; after the addition is completed, stir continuously for 3 hours in a constant temperature water bath at 80°C, and age for 1 hour to allow the precipitation to be fully formed; the precipitate is centrifuged, washed with deionized water, and dried to obtain a precursor; the precursor is placed in a muffle furnace at 3°C·min -1 The heating rate was heated from room temperature to 500 °C and maintained for 4 hours. After the heating was completed and cooled to room temperature, In 2 O 3 catalyst.
[0040] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1. Example 9
[0041] A method for preparing an In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol comprises the following steps: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M NH 3 ·H 2 O was added dropwise to the mixed solution using a peristaltic pump to adjust the pH of the mixed solution to 9; after the addition was completed, it was continuously stirred for 3 hours in a constant temperature water bath at 80°C and aged for 1 hour to allow the precipitation to fully form. The precipitate was centrifuged, washed with deionized water, and dried to obtain a precursor; the precursor was placed in a muffle furnace at 3°C·min -1 The heating rate was heated from room temperature to 700 °C and maintained for 4 hours. After the heating was completed and cooled to room temperature, In 2 O 3 catalyst.
[0042] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1.
[0043] Conclusion: Examples 1, 8, and 9 are about the regulation of the calcination temperature of the catalyst precursor during the preparation process. Appropriate calcination temperature can promote the formation of surface oxygen vacancies, which are usually one of the active sites of the catalyst. However, too high a calcination temperature may lead to the loss of oxygen vacancies or the formation of stable adsorbed oxygen, thereby affecting the activity of the catalyst. Comparative Example 1
[0044] A method for preparing an In2O3 catalyst comprises the following steps: adding 50 ml of deionized water and 3.0 g of indium nitrate pentahydrate into a round-bottom flask, stirring for 30 minutes until completely dissolved to form a mixed solution; taking an appropriate amount of 0.2 M (NH 4 ) 2 CO 3 , drop by drop into the mixed solution with a peristaltic pump, and adjust the pH of the mixed solution to 9; after the addition is completed, stir continuously for 3 hours in a constant temperature water bath at 80°C, and age for 1 hour to allow the precipitation to be fully formed; the precipitate is centrifuged, washed with deionized water, and dried to obtain a precursor; the precursor is placed in a muffle furnace at 3°C·min -1 The heating rate was heated from room temperature to 600 ° C, maintained for 4 hours, and after cooling to room temperature, In 2 O 3 catalyst.
[0045] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1. Comparative Example 2
[0046] A method for preparing an In2O3 catalyst, using N,N-dimethylformamide (DMF) as a pH regulator, comprising the following steps: adding 65 ml of N,N-dimethylformamide (DMF) and 3.2 ml of deionized water to a round-bottom flask, and performing a 500 r·min reaction at room temperature. -1The mixture was stirred at a high speed for 2 hours, and then transferred to a 100 ml stainless steel autoclave lined with polytetrafluoroethylene, and crystallized in an electric blast drying oven at 150°C for 24 hours. After the crystallization, the autoclave was taken out and naturally cooled to room temperature. The autoclave was opened, and the bottom precipitate was centrifuged and washed with deionized water. The mixture was stirred at 10000 r·min. -1 The product was centrifuged in a high-speed centrifuge for 10 minutes and washed with deionized water. The precipitate was then transferred to a 60°C vacuum drying oven and dried overnight to remove moisture and impurities to obtain a precursor. The precursor synthesized above was placed in a muffle furnace at 3°C min -1 The heating rate was set to 600 °C for 4 hours, and then In was obtained after cooling to room temperature. 2 O 3 catalyst.
[0047] This embodiment 2 O 3 The application of the catalyst sample in catalytic hydrogenation of carbon dioxide to methanol, the steps and process conditions are the same as those in Example 1. 2 O 3 Catalyst samples in CO 2 The performance evaluation conditions and results of the hydrogenation system for preparing methanol are shown in Appendix 1.
[0048] Conclusion: Compared with Example 1, Comparative Example 1 and Comparative Example 2 are two different preparation methods of In 2 O 3 Method. Example 1, Comparative Example 1 and Comparative Example 2 are respectively named In 2 O 3 -N、In 2 O 3 -A and In 2 O 3 -H, and their SEM images are Figure 1 , Figure 2 and Figure 3 In 2 O 3 -N has a flocculent structure and the smallest particle size (20nm); In 2 O 3 The rod-like structure of -A shows a different crystal growth pattern, with an average diameter of about 60nm; 2 O 3 -H has an elliptical shape and an average particle size of about 30nm. Figure 4 ) These three catalysts have the same crystal form, which is stable c-In 2 O 3 After N 2~ Adsorption-desorption test, In 2 O 3-N exhibited the largest specific surface area (50.34 m 2 / g), while In 2 O 3 -A and In 2 O 3 The specific surface areas of -H are 32.01m 2 / g and 21.78m 2 / g, compared to In 2 O 3 -H, In 2 O 3 -N increased by about two times. Further XPS analysis showed that the peaks at 529.9eV, 531.7eV, and 532.9eV represent the ionization potentials of lattice oxygen, oxygen vacancies, and adsorbed oxygen species, respectively. It is worth noting that In 2 O 3 -N surface oxygen vacancies (O defect ) concentration is 33%, slightly higher than In 2 O 3 -A(30%) and In 2 O 3 -H (28%). In summary, due to NH 3 ·H 2 O is alkaline, and its nucleation rate is faster than the crystal growth rate, so the formed In 2 O 3 Smaller particles have a larger specific surface area. This larger specific surface area is beneficial to CO 2 and H 2 The adsorption of oxygen vacancies promotes the formation of oxygen vacancies, making it an excellent CO 2 Performance of hydrogenation to methanol. Table 1 Catalyst CO 2 Evaluation conditions and performance of hydrogenation to methanol reaction
[0049] The above is only a preferred embodiment of the present invention, and should not be used to limit the scope of the present invention. That is, any simple equivalent changes and modifications made according to the scope of the patent application of the present invention and the content of the invention description are still within the scope of the patent of the present invention.
Claims
1. An In2O3 catalyst for catalyzing the hydrogenation of carbon dioxide to produce methanol, characterized in that: The indium salt is used as the raw material, a pH regulator is added and then calcined at 400-800°C.
2. The In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 1, characterized in that: The indium salt is In(NO3)3·5H2O.
3. The In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 1, characterized in that: The pH regulator is NH3·H2O or (NH4)2CO3.
4. The method for preparing the In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to any one of claims 1 to 3, characterized in that: The steps involved are as follows: (1) fully mixing indium salt and deionized water to obtain a mixed solution; (2) adding a pH adjuster to the mixed solution and adjusting the pH value of the mixed solution; (3) stirring continuously for 1 to 5 hours at a temperature of 70 to 90° C. and aging for 1 to 5 hours to form a precipitate; (4) preparing a precursor by centrifuging, washing, and drying the precipitate; (5) The precursor is placed in a muffle furnace, heated to 400-800°C and calcined in air.
5. The method for preparing an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 4, characterized in that: The concentration of the pH adjuster is 0.1M to 2M.
6. The method for preparing an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 4, characterized in that: Use a peristaltic pump to add pH regulator drop by drop, and the peristaltic pump drop rate is 1-10ml / min -1 .
7. The method for preparing the In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 4, characterized in that: The pH value ranges from 5 to 10.
8. An application of an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol in catalytic hydrogenation of carbon dioxide to methanol, characterized in that: The method comprises a reduction step and a catalytic step, wherein the catalytic reaction conditions of the catalytic step are: the reaction gas is a mixed gas composed of CO2:H2=1:2-1:4, and the air velocity is 5000-15000 ml·g -1 ·h -1 , the reaction temperature is 240-340°C, and the pressure is 2-6Mpa.
9. The use of an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to methanol according to claim 8 is characterized in that: The reduction conditions of the reduction step are as follows: reducing gas, a reduction temperature of 350° C., and a reduction time of 3 hours.
10. The use of an In2O3 catalyst for catalytic hydrogenation of carbon dioxide to produce methanol according to claim 8, characterized in that: The In2O3 catalyst should be sieved to a mesh size of 40 to 60 meshes.