Method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets, obtained product and application

By growing perovskite quantum dots on carbon nitride nanosheets by high-temperature solid-state method, the problem of ligand influence in the synthesis of perovskite quantum dots is solved, efficient photocatalytic performance is achieved, the range of photoresponse is expanded and the preparation time is reduced. Cost, suitable for the field of photocatalysis.

CN118754191AActive Publication Date: 2024-10-11UNIV OF JINAN
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410887993.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing perovskite quantum dot synthesis technology is difficult to obtain high-quality nanoparticles without ligands, which affects its application in the field of photocatalysis. Moreover, traditional methods require solution chemistry, resulting in low carrier transmission efficiency.

Method used

Perovskite quantum dots are grown in situ on carbon nitride nanosheets through a high-temperature solid-state method, using mechanochemical pre-reaction and thermal polymerization processes to ensure the formation of high-quality perovskite quantum dots/graphite phase nitridation under ligand-free conditions. Carbon composite materials realize the heterojunction of perovskite quantum dots and carbon nitride.

Benefits of technology

The carrier transmission efficiency and photocatalytic performance are improved, the photoresponse range is expanded, the preparation cost is reduced, and a perovskite quantum dot/graphite phase carbon nitride composite material with good crystallinity is obtained, which is suitable for photolysis of water and CO2 Photocatalytic reduction and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754191A_ABST
    Figure CN118754191A_ABST
Patent Text Reader

Abstract

The invention discloses a method for in-situ growth of perovskite quantum dots on a carbon nitride nanosheet, an obtained product and application, and the method comprises the following steps: mixing and grinding a perovskite quantum dot precursor and a graphite phase carbon nitride nanosheet to realize a mechanochemical pre-reaction; performing low-temperature freezing treatment, and calcining the frozen mixture in an inert atmosphere to realize in-situ synthesis of the perovskite quantum dots on the carbon nitride nanosheets; and sequentially carrying out water washing and alcohol washing on the calcined sample, and then drying to obtain the perovskite quantum dot / graphite phase carbon nitride nanosheet composite material. The quantum dots are directly synthesized under the high-temperature solid-phase condition, no ligand is added, the interface defects of the quantum dots and carbon nitride are few, carrier transport is facilitated, and the influence of the ligand on photon-generated carriers is eliminated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a composite method of perovskite quantum dots and carbon nitride nanosheets, and specifically to a method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets without the participation of ligands, in particular to a method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets by a high-temperature solid phase method, and also to the obtained perovskite quantum dot / graphite phase carbon nitride (g-C3N4) nanosheet composite material and the application of the composite material in the field of photocatalysis. Background Art

[0002] Graphitic carbon nitride is a typical visible light photocatalyst. It has been widely used in various photocatalytic fields in the past 20 years. It has attracted much attention because it does not contain metal elements, is non-toxic and environmentally friendly, inexpensive, and has a simple preparation process. In order to improve the performance of carbon nitride-based photocatalysts, expanding the light response and improving the separation and transmission efficiency of photogenerated carriers are key. Since layered carbon nitride materials can be prepared into ultra-thin nanosheets, forming a heterojunction with other semiconductor materials is the key to improving photocatalytic efficiency.

[0003] Perovskite quantum dots are a typical semiconductor luminescent material, whose light absorption can cover the entire visible light region. The luminescence process is exactly the opposite of photocatalysis. Luminescence is the emission of photons through the recombination of photogenerated electrons and holes, while the photocatalytic process is to achieve the separation of photogenerated electrons and holes. These photogenerated electrons and holes participate in the photocatalytic redox reaction respectively, so the luminescence phenomenon will disappear. Due to the excellent absorption properties of perovskite quantum dots, their application in the field of photocatalysis is obvious, and the key is to prevent the recombination of photogenerated electrons and holes. On the other hand, in order to obtain high-quality perovskite quantum dots, traditional solution chemistry methods usually require the addition of organic ligands to passivate the surface, and these ligands will affect the migration of photogenerated electrons. Therefore, the application of perovskite quantum dots to photocatalysts needs to be compounded under ligand-free conditions to obtain high-quality hydrophilic nanoparticles and well-developed interfaces. Summary of the invention

[0004] In view of the fact that the existing synthesis technology of perovskite quantum dots is difficult to be directly applied in the field of photocatalysis, the present invention provides a method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets. The method makes full use of the secondary high-temperature thermal polymerization process of carbon nitride, and directly embeds high-quality perovskite quantum dot nanocrystals in-situ into carbon nitride nanosheets by high-temperature solid-phase in-situ growth, thereby obtaining a heterojunction with excellent interface properties. The method is completed under high-temperature solid-phase conditions and does not require ligands, thereby ensuring the carrier transfer efficiency, and the secondary thermal polymerization of carbon nitride can also prevent the oxidation of perovskite quantum dots to ensure that its light absorption range is adjustable. The method has a simple process, good repeatability, and is conducive to industrial production. The prepared perovskite quantum dots are uniformly embedded in carbon nitride nanosheets, have good stability, and have good application prospects.

[0005] The specific technical solutions of the present invention are as follows: A method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets, the method comprising the following steps: (1) Mixing and grinding the perovskite quantum dot precursor and graphite phase carbon nitride nanosheets to achieve mechanochemical pre-reaction; (2) subjecting the mixture ground in step (1) to low-temperature freezing; (3) calcining the frozen sample under an inert atmosphere to achieve in-situ synthesis of perovskite quantum dots on carbon nitride nanosheets; (4) Washing and drying the calcined sample to obtain a perovskite quantum dot / graphite phase carbon nitride nanosheet composite material.

[0006] Furthermore, the structural formula of the perovskite quantum dots is CsPbX3, wherein X is a halogen, such as chlorine, bromine, iodine, and the like.

[0007] Furthermore, the precursor of the perovskite quantum dots is a mixture of cesium halide and lead halide, the cesium halide can be cesium chloride, cesium bromide, cesium iodide, etc., and the lead halide can be lead chloride, lead bromide, lead iodide, etc.

[0008] Furthermore, in step (1), the amounts of cesium halide and lead halide as perovskite quantum dot precursors are added according to the stoichiometric ratio of the perovskite quantum dot molecular formula.

[0009] Furthermore, in step (1), the total mass of the perovskite quantum dot precursor is 4-18 wt% of the graphite phase carbon nitride (g-C3N4) nanosheets, for example, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%.

[0010] Furthermore, in step (1), the perovskite quantum dot precursor and the graphite phase carbon nitride nanosheets are mixed and then fully ground, and the two are subjected to a mechanochemical pre-reaction by grinding. The mechanochemical pre-reaction refers to the pre-reaction of the precursor raw materials by grinding, and the raw materials are linked by hydrogen bonds.

[0011] Furthermore, in step (1), the mixture is ground until its volume expands to 1.2-1.5 times, for example, 1.2 times, 1.3 times, 1.4 times, 1.5 times, and grinding to this extent generally takes 4-10 hours, for example, 4h, 5h, 6h, 7h, 8h, 9h, 10h.

[0012] Furthermore, in step (2), the low-temperature freezing treatment is performed by freezing the mixture at -15 to -20°C for 4 to 6 hours, then thawing at room temperature, freezing the mixture at -15 to -20°C for 4 to 6 hours, and then thawing the mixture at room temperature.

[0013] Furthermore, in step (3), the mixture after low-temperature freezing treatment is calcined for a period of time at a certain temperature and in an inert atmosphere to complete the thermal polymerization of carbon nitride and realize the in-situ high-temperature solid-phase synthesis of quantum dots. The calcination temperature is 600-750°C, for example, 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C, 710°C, 720°C, 730°C, 740°C, 750°C. The insulation time is generally 10-40 minutes, for example, 10 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, 40 minutes.

[0014] Furthermore, in step (3), the inert atmosphere can be provided by an inert gas such as nitrogen or argon.

[0015] Furthermore, in step (3), the heating rate is generally 5-10°C / min.

[0016] Furthermore, in step (4), the calcined sample is first washed with water to remove unreacted chemical reagents, and the number of water washings is 1-5 times, for example, 1 time, 2 times, 3 times, 4 times, 5 times, preferably 3 times. After washing with water, it is then washed with ethanol 1-5 times, for example, 1 time, 2 times, 3 times, 4 times, 5 times, preferably 3 times.

[0017] The present invention also provides a perovskite quantum dot / graphite phase carbon nitride nanosheet composite material obtained according to the above method. The present invention realizes solid phase in-situ high temperature synthesis and growth of perovskite quantum dots on carbon nitride nanosheets through two processes of mechanochemical pre-reaction and high temperature thermal polymerization. The quantum dots have good crystallinity, form heterojunctions with graphite phase carbon nitride in the absence of ligands, and have better photocatalytic performance. The composite material obtained by the present invention is in the form of ultra-thin nanosheets, the thickness of the nanosheets is less than 1 nanometer, and the perovskite quantum dot nano-scale particles are uniformly embedded in the carbon nitride nanosheets.

[0018] The present invention also provides the application of the above-mentioned perovskite quantum dot / graphite phase carbon nitride nanosheet composite material in photocatalysis. The perovskite quantum dot / graphite phase carbon nitride nanosheet composite material can be used as a photocatalyst in the fields of photolysis of water to produce hydrogen, photocatalytic reduction of CO2, photocatalytic hydrogen peroxide production and chemical fuel conversion.

[0019] Compared with the prior art, the present invention has the following beneficial effects: 1. The present invention uses two processes, mechanical chemical prevention and high temperature thermal polymerization, to achieve solid phase in-situ high temperature synthesis and growth of perovskite quantum dots on carbon nitride nanosheets. By controlling the reaction process and the ratio of the two phases, the light absorption of the obtained composite material is expanded to the entire visible light range, and a photocatalyst with good performance is obtained.

[0020] 2. The quantum dots of the present invention are directly synthesized under high-temperature solid-phase conditions without the addition of ligands. The quantum dots have good crystallinity, and the interface defects between the quantum dots and carbon nitride are few, which is beneficial to carrier transport. At the same time, the ligands required for solution chemical synthesis are not required, which eliminates the influence of the ligands on photogenerated carriers, expands the light absorption of carbon nitride materials, expands the light response range, improves the utilization rate of sunlight, improves the separation and conversion efficiency of photogenerated carriers, and improves the photocatalytic performance of carbon nitride.

[0021] 3. The preparation method of the present invention is simple, easy to implement, does not use organic solvents, and has low manufacturing costs. The obtained perovskite quantum dot / graphite phase carbon nitride nanosheet composite material has important application prospects in the fields of photolysis of water to produce hydrogen, photocatalytic reduction of CO2, photocatalytic hydrogen peroxide production and chemical fuel conversion. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is an electron microscope photograph of the sample obtained in Example 1.

[0023] Figure 2 This is a graph showing the stability cycle test results of the photolysis of water to produce hydrogen for the sample obtained in Example 1. DETAILED DESCRIPTION

[0024] The present invention is further described below by way of examples. The following description is only for explaining the present invention and is not intended to limit its contents.

[0025] In the following examples, the g-C3N4 nanosheets used were purchased from Suzhou Beike Nanotechnology Co., Ltd.

[0026] Example 1 1.1 Add 1.74 g of commercial g-C3N4 nanosheet powder, 0.11 g of lead bromide, 0.064 g of cesium bromide, and 2 mL of ethanol into an agate mortar and grind in one direction until the solvent evaporates completely; after the solvent evaporates, add the solvent again and continue grinding in the same way. Grind for 8 hours in the above manner until the volume expands to 1.3 times the original volume.

[0027] 1.2 Freeze the above samples at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature. After thawing, freeze them again at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature.

[0028] 1.3 Take the sample obtained in step 1.2, heat it to 700℃ at a heating rate of 7℃ / min under nitrogen atmosphere and keep it for 30 minutes, then grind the sample into fine powder for later use.

[0029] 1.4 Take the sample from step 1.3, wash it with water and ethanol three times respectively, and then dry it to obtain the CsPbBr3 / g-C3N4 composite photocatalyst. Figure 1 This is a transmission electron microscope photograph of the obtained sample. It can be seen from the figure that the sample is in a flake shape, and the cesium lead bromide nanoparticles are uniformly embedded in the carbon nitride nanosheets and are evenly distributed. Figure 1 The middle inset is an enlarged electron microscope photograph of a cesium lead bromide nanoparticle. A clear lattice phase can be observed from the inset, indicating that the cesium lead bromide quantum dots have good crystallinity.

[0030] Example 2 2.1 Add 4.35 g of commercial g-C3N4 nanosheet powder, 0.11 g of lead bromide, 0.064 g of cesium bromide, and 2 mL of ethanol into an agate mortar and grind in one direction until the solvent evaporates completely; after the solvent evaporates, add the solvent again and continue grinding in the same way. Grind in the above way for 4 hours until the volume expands to 1.2 times the original volume.

[0031] 2.2 Freeze the above samples at -15 degrees Celsius for 6 hours and then thaw naturally at room temperature. After thawing, freeze them again at -15 degrees Celsius for 6 hours and then thaw naturally at room temperature.

[0032] 2.3 Take the sample obtained in step 2.2, heat it to 600℃ at a heating rate of 5℃ / min under nitrogen atmosphere and keep it for 40 minutes, then grind the sample into fine powder for later use.

[0033] 2.4 Take the sample from step 2.3, wash it with water and ethanol three times respectively, and dry it to obtain the CsPbBr3 / g-C3N4 composite photocatalyst. The morphology of the obtained sample is similar to that of Example 1.

[0034] Example 3 3.1 Add 0.97 g of commercial g-C3N4 nanosheet powder, 0.11 g of lead bromide, 0.064 g of cesium bromide, and 2 mL of ethanol into an agate mortar and grind in one direction until the solvent evaporates completely; after the solvent evaporates, add the solvent again and continue grinding in the same way. Grind for 10 hours in the above manner until the volume expands to 1.5 times the original volume.

[0035] 3.2 Freeze the above samples at -20 degrees Celsius for 4 hours and then thaw naturally at room temperature. After thawing, freeze them again at -20 degrees Celsius for 4 hours and then thaw naturally at room temperature.

[0036] 3.3 Take the sample obtained in step 3.2, heat it to 750℃ at a heating rate of 10℃ / min under nitrogen atmosphere and keep it for 10 minutes, then grind the sample into fine powder for later use.

[0037] 3.4 Take the sample from step 3.3, wash it with water and ethanol three times respectively, and dry it to obtain the CsPbBr3 / g-C3N4 composite photocatalyst. The morphology of the obtained sample is similar to that of Example 1.

[0038] Example 4 4.1 Add 1.36 g of commercial g-C3N4 nanosheet powder, 0.086 g of lead chloride, 0.05 g of cesium chloride, and 2 mL of ethanol into an agate mortar and grind in one direction until the solvent evaporates completely; after the solvent evaporates, add the solvent again and continue grinding in the same way. Grind in the above way until the volume expands to 1.3 times the original volume.

[0039] 4.2 Freeze the above samples at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature. After thawing, freeze them again at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature.

[0040] 4.3 Take the sample obtained in step 4.2, heat it to 700℃ at a heating rate of 7℃ / min under nitrogen atmosphere and keep it for 30 minutes, then grind the sample into fine powder for later use.

[0041] 4.4 Take the sample of step 4.3, wash it with water and ethanol three times respectively, and obtain the CsPbCl3 / g-C3N4 composite photocatalyst after drying. The morphology of the obtained sample is similar to that of Example 1, and the photocatalytic hydrogen production performance is about 85% of that of Example 1. The reason is that the absorption wavelength of cesium lead chloride quantum dots becomes shorter and the absorption of visible light becomes narrower.

[0042] Example 5 5.1 Add 2.18 g of commercial g-C3N4 nanosheet powder, 0.14 g of lead iodide, 0.078 g of cesium iodide, and 2 mL of ethanol into an agate mortar and grind in one direction until the solvent evaporates completely; after the solvent evaporates, add the solvent again and continue grinding in the same way. Grind in the above way until the volume expands to 1.3 times the original volume.

[0043] 5.2 Freeze the above samples at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature. After thawing, freeze them again at -18 degrees Celsius for 5 hours and then thaw naturally at room temperature.

[0044] 5.3 Take the sample obtained in step 5.2, heat it to 700℃ at a heating rate of 7℃ / min under nitrogen atmosphere and keep it for 30 minutes, then grind the sample into fine powder for later use.

[0045] 5.4 Take the sample of step 5.3, wash it with water and ethanol three times respectively, and dry it to obtain CsPbI3 / g-C3N4 composite photocatalyst. The morphology of the obtained sample is similar to that of Example 1, and the photocatalytic hydrogen production performance is about 104% of that of Example 1. The reason is that the absorption wavelength of cesium lead iodide quantum dots becomes longer, the absorption region of visible light becomes wider, and the efficiency is improved.

[0046] Example 6 The CsPbBr3 / g-C3N4 composite photocatalyst was prepared according to the method of Example 1, except that in step 1.1, the amount of lead bromide used was 0.044 g and the amount of cesium bromide used was 0.0256 g. The morphology of the obtained sample was similar to that of Example 1, and the photocatalytic hydrogen production performance was about 70% of that of Example 1.

[0047] Example 7 The CsPbBr3 / g-C3N4 composite photocatalyst was prepared according to the method of Example 1, except that in step 1.1, the amount of lead bromide used was 0.198 g and the amount of cesium bromide used was 0.115 g. The morphology of the obtained sample was similar to that of Example 1, and the photocatalytic hydrogen production performance was about 60% of that of Example 1.

[0048] Comparative Example 1 1.1 Add 1.74 g of g-C3N4 powder, 0.11 g of lead bromide, 0.064 g of cesium bromide, and 2 mL of ethanol into an agate mortar and grind in one direction. After the solvent is completely evaporated, add the solvent and continue grinding. Stop grinding after 2 hours. The mixture does not expand in volume. 1.2 Same as Example 1.2; 1.3 Same as Example 1.3; 1.4 Same as Example 1.4; Electron microscope photos show that the cesium lead bromide quantum dots in the obtained sample are unevenly distributed on the carbon nitride, and the quantum dots and carbon nitride are not well composited. The photocatalytic performance is very poor, similar to pure carbon nitride, and the two materials on the surface are not well composited.

[0049] Comparative Example 2 The product was prepared in the same manner as in Example 2, except that in step 2.3, the temperature was raised to 800°C at a rate of 5°C / min under a nitrogen atmosphere and kept at that temperature for 20 minutes. The results showed that the sample was black and had almost no photocatalytic hydrogen production properties.

[0050] Comparative Example 3 The product was prepared in the manner of Example 3, except that step 3.2 was omitted and the ground sample was directly calcined.

[0051] The results showed that the looseness of the sample deteriorated and some of them agglomerated. The sample could not be evenly dispersed during the photolysis of water and the photocatalytic properties were poor.

[0052] Photocatalytic performance verification Photocatalytic water hydrogen production experiments were carried out using the samples of the embodiments and comparative examples as photocatalysts. The experiments were carried out in conventional water system hydrogen production equipment. The light source was a full-spectrum xenon lamp. The irradiation light source was controlled in the visible light region by a filter. The catalyst was added to the reactor, and 1% chloroplatinic acid solution was added dropwise as a co-catalyst. The catalyst was the photocatalyst prepared in the above embodiments and comparative examples, commercially available CsPbBr3 quantum dots, or the g-C3N4 nanosheet powder in step 1.1 of embodiment 1.

[0053] The hydrogen production was detected by gas chromatography, and then the hydrogen production rate at 2.5 h was calculated. The hydrogen production rate formula was: molar amount of hydrogen / (mass of catalyst × 2.5 h). The results are shown in Table 1.

[0054] The stability experiment was carried out using the photocatalyst of Example 1 as an example. The experimental steps were as shown above. The hydrogen production time was 2.5 hours each time. The experiment was repeated 4 times in total. The catalyst used in the first experiment was used in the subsequent experiments. The experimental results are shown in Figure 2. Figure 2 As shown in the figure, it can be seen that the hydrogen production efficiency of the catalyst has not decreased after 4 tests, indicating that the photocatalyst of the present invention has good cyclability stability.

Claims

1. A method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets, characterized in that The following steps are involved: (1) Mixing and grinding the perovskite quantum dot precursor and graphite phase carbon nitride nanosheets to achieve mechanochemical pre-reaction; (2) subjecting the mixture ground in step (1) to low-temperature freezing; (3) calcining the frozen sample under an inert atmosphere to achieve in-situ synthesis of perovskite quantum dots on carbon nitride nanosheets; (4) Washing and drying the calcined sample to obtain a perovskite quantum dot / graphite phase carbon nitride nanosheet composite material.

2. The method according to claim 1, characterized in that: The perovskite quantum dot structural formula is CsPbX3, wherein X is a halogen.

3. The method according to claim 1, characterized in that: The precursor of perovskite quantum dots is a mixture of cesium halide and lead halide.

4. The method according to claim 1 or 3, characterized in that: The amount of perovskite quantum dot precursor used is 4-18 wt% of graphite phase carbon nitride nanosheets.

5. The method according to claim 1, characterized in that: In step (1), the mixture is ground until its volume expands to 1.2-1.5 times of its original volume; preferably, the grinding time is 4-10 hours.

6. The method according to claim 1, characterized in that: In step (2), the low-temperature freezing treatment is performed by freezing the mixture at -15 to -20°C for 4 to 6 hours, then thawing at room temperature, freezing the mixture at -15 to -20°C for 4 to 6 hours, and then thawing the mixture at room temperature.

7. The method according to claim 1, characterized in that: In step (3), the calcination temperature is 600-750°C and the holding time is 10-40 minutes.

8. The method according to claim 1 or 7, characterized in that: In step (3), the heating rate is 5-10°C / min.

9. The method according to claim 1, characterized in that: In step (4), during washing, water washing is performed first, and then alcohol washing is performed.

10. A perovskite quantum dot / graphite phase carbon nitride nanosheet composite material and its use as a photocatalyst, characterized by: The perovskite quantum dot / graphite phase carbon nitride nanosheet composite material is obtained by the method for in-situ growth of perovskite quantum dots on carbon nitride nanosheets as described in any one of claims 1-9.

Citation Information

Patent Citations

  • P-CN / CsPbBr3 heterojunction material, and preparation method and application thereof

    CN112121837A

  • All-inorganic lead halide perovskite quantum dot and zeolite composite luminescent material and preparation method thereof

    CN114276798A

  • Lead-free perovskite-loaded graphene-like carbon nitride visible-light-driven photocatalyst and preparation method thereof

    CN115445641A

  • In-situ generated perovskite heterojunction photocatalyst, preparation method and application

    CN115569659A

  • Perovskite quantum dot MOFs composite luminescent material suitable for water environment and preparation method thereof

    CN118185627A