Corrosion-resistant seamless steel tube and preparation method thereof

Through corrosion-resistant coatings combined with graphite phase carbon nitride and silica, a barrier layer is formed and self-repair is achieved, which solves the problem of corrosion of seamless steel pipes in underground drilling environments, and significantly improves its corrosion resistance and service life.

CN119039852APending Publication Date: 2024-11-29NANTONG HONGYUAN GEOLOGICAL ENG MATERIAL

Patent Information

Application Number
CN202411159659.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Seamless steel pipes are susceptible to moisture, acid and alkalinity and microorganisms in underground drilling environments, resulting in damage, and the prior art is difficult to effectively improve their corrosion resistance.

Method used

Corrosion-resistant coatings that combine graphite phase carbon nitride and silica are used to form a barrier layer through the mesh structure of graphite phase carbon nitride and the fixation of silica, which prevents the diffusion of corrosive electrolytes and passes through benzotrinitrogen. The loads achieve self-healing effect of the coating.

Benefits of technology

It significantly improves the corrosion resistance of steel pipes and extends its service life in corrosion environments, especially in brine, acidic and alkaline conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119039852A_ABST
    Figure CN119039852A_ABST
Patent Text Reader

Abstract

The invention relates to a corrosion-resistant seamless steel pipe and a preparation method thereof, and relates to the technical field of steel pipe materials. The corrosion-resistant seamless steel pipe comprises a steel pipe body, a corrosion-resistant coating is arranged on the surface of the steel pipe body, the corrosion-resistant coating is obtained by coating the surface of the steel pipe body with corrosion-resistant paint, and the corrosion-resistant paint comprises, by mass, 55%-60% of epoxy resin, 13%-17% of graphite phase carbon nitride, 0.8%-1.2% of auxiliaries and the balance butyl acetate which is filled to 100%. The effect of improving the corrosion resistance of the seamless steel pipe is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of steel pipe materials, and in particular to a corrosion-resistant seamless steel pipe and a preparation method thereof. Background Art

[0002] Seamless steel pipes are divided into hot-rolled seamless steel pipes and cold-rolled seamless steel pipes, and cold-rolled pipes are divided into round pipes and special-shaped pipes. As the technology of drilling exploration becomes more and more mature, the drill pipe formed by seamless steel pipes is an important part of geological exploration equipment, and its use is also increasing.

[0003] Seamless steel pipes are usually made of a mixture of pig iron, refining agents and alloy doping components. When seamless steel pipes need to be used deep underground, the underground environment is complex. It not only has a high moisture content, but also has high acidity and alkalinity, and more microorganisms, which will cause long-term corrosion to the seamless steel pipes and cause damage to the seamless steel pipes. Summary of the invention

[0004] In order to improve the corrosion resistance of seamless steel pipes, the present application provides a corrosion-resistant seamless steel pipe and a preparation method thereof.

[0005] In the first aspect, the present application provides a corrosion-resistant seamless steel pipe, which adopts the following technical solution: A corrosion-resistant seamless steel pipe comprises a steel pipe body, the surface of the steel pipe body is provided with a corrosion-resistant coating, the corrosion-resistant coating is obtained by applying the corrosion-resistant coating to the surface of the steel pipe body, the corrosion-resistant coating comprises the following components in mass percentage: 55-60% epoxy resin, 13-17% graphite phase carbon nitride, 0.8-1.2% additive, and the rest is filled with butyl acetate to 100%.

[0006] By adopting the above technical solution, the corrosion-resistant coating produced by using graphite phase carbon nitride as one of the raw materials is coated on the surface of the steel pipe body, so that the steel pipe body has excellent corrosion resistance and good practical effect. The specific solution analysis is as follows: Graphite carbon nitride is a two-dimensional nanomaterial with excellent ion impermeability and chemical stability. When graphite carbon nitride is added to the coating, it can fill the network structure formed after the epoxy resin is cured, prolong the penetration process of corrosive electrolytes inside the coating, and then establish a physical barrier between the steel pipe body and the corrosive substances, so as to play a corrosion-resistant role through the barrier properties of the coating itself.

[0007] In addition, graphite phase carbon nitride also has photocatalytic activity, which can produce more photogenerated oxidative active substances, thereby destroying the cell structure to achieve the purpose of blocking bacterial attachment, thereby improving the corrosion resistance of the steel pipe body.

[0008] Preferably, the graphite phase carbon nitride is prepared by the following steps: The graphite phase carbon nitride, silicon dioxide and ethanol are mixed and stirred evenly, and then ethanol, deionized water and ammonia water are added, heated and stirred evenly, and then filtered, washed and dried to obtain modified graphite phase carbon nitride.

[0009] By adopting the above technical solution, due to the poor compatibility of graphite phase carbon nitride with epoxy resin, the graphite phase carbon nitride has a poor filling effect on the tiny gaps in the coating, and the graphite phase carbon nitride itself is prone to agglomeration, resulting in a decrease in the corrosion resistance of the corrosion-resistant coating.

[0010] Therefore, the graphite phase carbon nitride is combined with silicon dioxide so that the silicon dioxide is fixed on the graphite phase carbon nitride, thereby inhibiting the aggregation of the graphite phase carbon nitride in the epoxy resin, and providing rich oxygen-containing functional groups, thereby improving the interfacial bonding strength between the graphite phase carbon nitride and the epoxy resin, thereby blocking the diffusion path of the corrosive electrolyte, improving the corrosion resistance of the corrosion-resistant coating, and then improving the corrosion resistance of the steel pipe body.

[0011] At this time, silica has good heat resistance, chemical resistance and corrosion resistance, so silica plays a positive role in improving the corrosion resistance of the steel pipe body.

[0012] Preferably, benzotriazole is added during the modification process of the graphite phase carbon nitride, that is, the modification preparation steps of the graphite phase carbon nitride are as follows: S100, mixing graphite phase carbon nitride, silicon dioxide and ethanol, stirring evenly, then adding ethanol, deionized water and ammonia water, heating and stirring evenly, filtering, washing and drying to obtain primary modified graphite phase carbon nitride; S200, adding primary modified graphite phase carbon nitride to an aqueous solution of tris(hydroxymethyl)aminomethane hydrochloride; then adding benzotriazepine dissolved in anhydrous ethanol and finally adding a binder, stirring evenly, centrifuging and drying to obtain modified graphite phase carbon nitride.

[0013] By adopting the above technical scheme, the co-adsorption effect of the binder is used to promote the loading of benzotriazepine on the graphite phase carbon nitride, so that when the corrosive medium penetrates into the surface of the steel pipe body, the benzotriazepine can react with the corrosion product to form a film layer on the surface of the steel pipe body. Therefore, when the corrosive medium reaches the surface of the steel pipe body, the steel pipe body can still be continuously protected, and the self-repairing effect of the coating after damage is achieved, thereby improving the corrosion resistance of the steel pipe body.

[0014] Preferably, the mass ratio of the graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:(3.2-3.6):(2.1-2.5).

[0015] By adopting the above technical solution, the mass ratio of graphite phase carbon nitride, silicon dioxide and benzotriazole is controlled within the above range, which can effectively improve the corrosion resistance of the corrosion-resistant coating.

[0016] Preferably, the binder is dopamine.

[0017] By adopting the above technical solution, dopamine can effectively improve the tightness of the combination of silicon dioxide and graphite phase carbon nitride, and promote the loading of benzotriazole on graphite phase carbon nitride.

[0018] Preferably, the silicon dioxide is prepared by the following steps: Silicon dioxide is added to anhydrous ethanol, and after ultrasonic treatment, trimethylchlorosilane is added, and after heating reaction, centrifugation is performed, and then the product is washed, dried, and ground to obtain modified silicon dioxide.

[0019] By adopting the above technical scheme, the hydroxyl groups on the surface of silica react with trimethylchlorosilane to generate silanols, and interact through hydrogen bonds, so that the silanols are grafted onto the surface of silica. As a result, the polar hydroxyl groups on the surface of silica are replaced by non-polar methyl groups through silanization of silica, so that the hydrophobicity of silica is improved, thereby improving the corrosion resistance of silica.

[0020] Preferably, the mass ratio of silicon dioxide to trimethylchlorosilane is 1:(0.17-0.21).

[0021] By adopting the above technical solution and controlling the mass ratio of silicon dioxide to trimethylchlorosilane within the above range, the hydrophobicity of silicon dioxide can be effectively improved.

[0022] Preferably, the epoxy resin is bisphenol A epoxy resin.

[0023] Preferably, the auxiliary agent is formed by mixing silicone, polythiol and polyamide.

[0024] In a second aspect, the present application provides a method for preparing a corrosion-resistant seamless steel pipe as in the first aspect, which adopts the following technical solution: Preferably, a method for preparing a corrosion-resistant seamless steel pipe comprises the following steps: S1. Mix graphite phase carbon nitride and butyl acetate and stir evenly, then add epoxy resin and additives, stir evenly, and let stand to prepare a corrosion-resistant coating; S2. Apply the corrosion-resistant coating to the surface of the steel pipe body, and after curing, obtain a corrosion-resistant seamless steel pipe.

[0025] In summary, the present application includes at least one of the following beneficial technical effects: 1. Graphite carbon nitride is a two-dimensional nanomaterial with excellent ion impermeability and chemical stability. When graphite carbon nitride is added to the coating, it can fill the network structure formed after the epoxy resin is cured, prolong the penetration process of the corrosive electrolyte inside the coating, and then establish a physical barrier between the steel pipe body and the corrosive substance, so as to play a corrosion-resistant role through the barrier properties of the coating itself.

[0026] 2. The graphite phase carbon nitride is combined with silicon dioxide so that silicon dioxide is fixed on the graphite phase carbon nitride, thereby inhibiting the aggregation of graphite phase carbon nitride in the epoxy resin, and providing rich oxygen-containing functional groups, thereby improving the interfacial bonding strength between the graphite phase carbon nitride and the epoxy resin, thereby blocking the diffusion path of the corrosive electrolyte, improving the corrosion resistance of the corrosion-resistant coating, and then improving the corrosion resistance of the steel pipe body. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the overall structure of a seamless steel pipe in an embodiment of the present application.

[0028] Description of reference numerals: 1. Steel pipe body; 2. Corrosion-resistant layer. DETAILED DESCRIPTION

[0029] The following is combined with Figure 1 This application is described in further detail.

[0030] The present application discloses a corrosion-resistant seamless steel pipe. Figure 1 The corrosion-resistant seamless steel pipe comprises a steel pipe body 1 , and a corrosion-resistant coating 2 is arranged on the surface of the steel pipe body 1 . The corrosion-resistant coating 2 is obtained by coating the corrosion-resistant coating on the surface of the steel pipe body 1 .

[0031] The present application is further described in detail below in conjunction with the examples and comparative examples. The raw materials involved in the present application can be obtained commercially, and the polyamide is provided by Shanghai MacLean Biochemical Technology Co., Ltd.

[0032] Example 1 The corrosion-resistant coating includes the following components by weight: 55 g of epoxy resin, 13 g of graphite phase carbon nitride, 0.8 g of an auxiliary agent, and 31.2 g of butyl acetate.

[0033] The epoxy resin is bisphenol A epoxy resin, and the auxiliary agent is formed by mixing silicone, polythiol and polyamide, wherein the mass ratio of silicone, polythiol and polyamide is 1:1:1.

[0034] A method for preparing a corrosion-resistant seamless steel pipe comprises the following steps: S1. Mix graphite phase carbon nitride and butyl acetate and stir evenly, then add epoxy resin and additives, stir for 30 minutes, and then stand for 30 minutes to prepare a corrosion-resistant coating; S2. Apply the corrosion-resistant coating to the surface of the steel pipe body and dry it at 20°C for 72 hours to obtain a corrosion-resistant seamless steel pipe.

[0035] Example 2 The corrosion-resistant coating includes the following components by weight: 60 g of epoxy resin, 17 g of graphite phase carbon nitride, 1.2 g of an auxiliary agent, and 21.8 g of butyl acetate.

[0036] The epoxy resin is bisphenol A epoxy resin, and the auxiliary agent is formed by mixing silicone, polythiol and polyamide, wherein the mass ratio of silicone, polythiol and polyamide is 1:1:1.

[0037] A method for preparing a corrosion-resistant seamless steel pipe comprises the following steps: S1. Mix graphite phase carbon nitride and butyl acetate, stir evenly, add epoxy resin and additives, stir for 30 minutes, and then stand for 30 minutes to prepare a corrosion-resistant coating; S2. Apply the corrosion-resistant coating to the surface of the steel pipe body and dry it at 20°C for 72 hours to obtain a corrosion-resistant seamless steel pipe.

[0038] Example 3 The corrosion-resistant coating comprises the following components by weight: 58 g of epoxy resin, 15 g of graphite phase carbon nitride, 1 g of an auxiliary agent, and 26 g of butyl acetate.

[0039] The epoxy resin is bisphenol A epoxy resin, and the auxiliary agent is formed by mixing silicone, polythiol and polyamide, wherein the mass ratio of silicone, polythiol and polyamide is 1:1:1.

[0040] A method for preparing a corrosion-resistant seamless steel pipe comprises the following steps: S1. Mix graphite phase carbon nitride and butyl acetate, stir evenly, add epoxy resin and additives, stir for 30 minutes, and then stand for 30 minutes to prepare a corrosion-resistant coating; S2. Apply the corrosion-resistant coating to the surface of the steel pipe body and dry it at 20°C for 72 hours to obtain a corrosion-resistant seamless steel pipe.

[0041] Example 4 The difference between Example 4 and Example 3 is that the graphite phase carbon nitride is prepared by the following steps: 0.1 g of graphite phase carbon nitride, 3.2 g of silicon dioxide and 60 g of ethanol were mixed, stirred for 25 minutes, and then 60 g of ethanol, 20 g of deionized water and 2 g of ammonia water were added, stirred at 40°C for 4 hours, and then filtered. The product was washed with deionized water to remove impurities, and dried in an oven at 60°C for 12 hours to obtain modified graphite phase carbon nitride.

[0042] Example 5 The difference between Example 5 and Example 4 is that benzotriazole is also added during the modification process of graphite phase carbon nitride. The modification preparation steps of graphite phase carbon nitride are as follows: S100, 0.1g of graphite phase carbon nitride, 3.2g of silicon dioxide, and 60g of ethanol were mixed, stirred for 25min, and then 60g of ethanol, 20g of deionized water, and 2g of ammonia water were added, stirred at 40°C for 4h, and then filtered, the product was washed with deionized water to remove impurities, and then dried in an oven at 60°C for 12h to obtain primary modified graphite phase carbon nitride; S200, adding the primary modified graphite phase carbon nitride to 200g of tris(hydroxymethyl)aminomethane hydrochloride aqueous solution (the pH of the tris(hydroxymethyl)aminomethane hydrochloride aqueous solution is 8.5); then adding 2.5g of benzotriazepine dissolved in 50g of anhydrous ethanol and finally adding 1.2g of a binder, stirring for 24h, centrifuging three times with deionized water, and then drying in a 60°C oven for 12h to obtain modified graphite phase carbon nitride.

[0043] The binder is dopamine.

[0044] Example 6 The difference between Example 6 and Example 4 is that benzotriazole is also added during the modification process of graphite phase carbon nitride. The modification preparation steps of graphite phase carbon nitride are as follows: S100, 0.1g of graphite phase carbon nitride, 3.6g of silicon dioxide, and 60g of ethanol were mixed, stirred for 25min, and then 60g of ethanol, 20g of deionized water, and 2g of ammonia water were added, stirred at 40°C for 4h, and then filtered, the product was washed with deionized water to remove impurities, and then dried in an oven at 60°C for 12h to obtain primary modified graphite phase carbon nitride; S200, adding the primary modified graphite phase carbon nitride to 200g of tris(hydroxymethyl)aminomethane hydrochloride aqueous solution (the pH of the tris(hydroxymethyl)aminomethane hydrochloride aqueous solution is 8.5); then adding 2.1g of benzotriazepine dissolved in 50g of anhydrous ethanol and finally adding 1.2g of a binder, stirring for 24h, centrifuging three times with deionized water, and then drying in a 60°C oven for 12h to obtain modified graphite phase carbon nitride.

[0045] The binder is dopamine.

[0046] Example 7 The difference between Example 7 and Example 4 is that benzotriazole is also added during the modification process of graphite phase carbon nitride. The modification preparation steps of graphite phase carbon nitride are as follows: S100, 0.1 g of graphite phase carbon nitride, 3.4 g of silicon dioxide, and 60 g of ethanol were mixed, stirred for 25 min, and then 60 g of ethanol, 20 g of deionized water, and 2 g of ammonia water were added, stirred at 40 ° C for 4 h, and then filtered, the product was washed with deionized water to remove impurities, and then dried in an oven at 60 ° C for 12 h to obtain primary modified graphite phase carbon nitride; S200, adding the primary modified graphite phase carbon nitride to 200g of tris(hydroxymethyl)aminomethane hydrochloride aqueous solution (the pH of the tris(hydroxymethyl)aminomethane hydrochloride aqueous solution is 8.5); then adding 2.3g of benzotriazepine dissolved in 50g of anhydrous ethanol and finally adding 1.2g of a binder, stirring for 24h, centrifuging three times with deionized water, and then drying in a 60°C oven for 12h to obtain modified graphite phase carbon nitride.

[0047] The binder is dopamine.

[0048] Example 8 The difference between Example 8 and Example 7 is that the mass ratio of graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:2.4:1.8.

[0049] Example 9 The difference between Example 9 and Example 7 is that the mass ratio of graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:2.4:2.8.

[0050] Example 10 The difference between Example 10 and Example 7 is that the mass ratio of graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:2.8:2.4.

[0051] Embodiment 11 The difference between Example 11 and Example 7 is that the mass ratio of graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:4.0:2.4.

[0052] Example 12 The difference between Example 12 and Example 7 is that the silicon dioxide is prepared by the following steps: 10 g of silica was added to 400 g of anhydrous ethanol, and after ultrasonic treatment for 15 minutes, 1.7 g of trimethylsilyl chloride was added, and the mixture was reacted at 50° C. for 16 hours. The mixture was centrifuged at 10,000 r / min for 10 minutes, and then washed twice with anhydrous ethanol. The mixture was then dried at a constant temperature of 60° C. for 24 hours, and the modified silica was obtained after sufficient grinding.

[0053] Example 13 The difference between Example 13 and Example 7 is that the silicon dioxide is prepared by the following steps: 10 g of silica was added to 400 g of anhydrous ethanol, and after ultrasonic treatment for 15 minutes, 2.1 g of trimethylsilyl chloride was added, and the mixture was reacted at 50° C. for 16 hours. The mixture was centrifuged at 10,000 r / min for 10 minutes, and then washed twice with anhydrous ethanol. The mixture was then dried at a constant temperature of 60° C. for 24 hours, and the modified silica was obtained after sufficient grinding.

[0054] Embodiment 14 The difference between Example 14 and Example 7 is that the silicon dioxide is prepared by the following steps: 10 g of silica was added to 400 g of anhydrous ethanol, and after ultrasonic treatment for 15 minutes, 1.9 g of trimethylsilyl chloride was added, and the mixture was reacted at 50° C. for 16 hours. The mixture was centrifuged at 10,000 r / min for 10 minutes, and then washed twice with anhydrous ethanol. The mixture was then dried at a constant temperature of 60° C. for 24 hours, and the modified silica was obtained after sufficient grinding.

[0055] Embodiment 15 The difference between Example 15 and Example 12 is that the mass ratio of silicon dioxide to trimethylchlorosilane is 1:0.14.

[0056] Example 16 The difference between Example 16 and Example 12 is that the mass ratio of silicon dioxide to trimethylchlorosilane is 1:0.24.

[0057] Comparative Example 1 The difference between Comparative Example 1 and Example 3 is that no corrosion-resistant coating is provided on the surface of the steel pipe body.

[0058] Performance testing: 1. Corrosion resistance test: (1) Salt water resistance test The steel pipe coated with the coating was sampled five times, and the time required for complete corrosion under the condition of 20% NaCl was calculated. The results were averaged and the test results were recorded in Table 1.

[0059] (2) Acid resistance test The steel pipe coated with the coating was sampled five times, and the time required for complete corrosion under the condition of 50% concentrated sulfuric acid was calculated. The results were averaged and the test results were recorded in Table 1.

[0060] (3) Alkali resistance test The steel pipe coated with the coating was sampled five times, and the time required for complete corrosion under the condition of 10% NaOH was calculated. The results were averaged and the test results were recorded in Table 1.

[0061] Table 1 Data analysis Specifically combining the test results of Examples 1-3 and 4, the salt resistance of Examples 1-3 is >2472h, the acid resistance is >1989h, and the alkali resistance is >2132h, and the salt resistance of Example 4 is >2827h, the acid resistance is >2434h, and the alkali resistance is >2563h. It can be seen that the corrosion resistance of Example 4 is better than that of Examples 1-3. The analysis is as follows: The difference between Example 4 and Example 1-3 is that silicon dioxide is added during the preparation process of graphite phase carbon nitride modification. On the one hand, silicon dioxide itself has excellent corrosion resistance. On the other hand, by fixing silicon dioxide on graphite phase carbon nitride, the interface bonding strength between graphite phase carbon nitride and epoxy resin is improved, thereby improving the corrosion resistance of the corrosion-resistant coating, and then improving the corrosion resistance of the steel pipe body.

[0062] Specifically combining the test results of Example 4 and Example 5-7, the salt resistance of Example 4 is >2827h, the acid resistance is >2434h, and the alkali resistance is >2563h, and the salt resistance of Example 5-7 is >3544h, the acid resistance is >3170h, and the alkali resistance is >3247h. It can be seen that the corrosion resistance of Example 5-7 is better than that of Example 4. The analysis is as follows: The difference between Example 5-7 and Example 4 is that benzotriazole is added during the preparation process of graphite phase carbon nitride modification so that benzotriazole loads graphite phase carbon nitride, thereby realizing the self-repairing effect of the corrosion-resistant coating after damage, thereby improving the corrosion resistance of the steel pipe body.

[0063] Specifically combining the test results of the implementation of graphite phase carbon nitride examples 12-14 and Example 7, the salt resistance of Example 12-14 is >3876h, the acid resistance is >3425h, and the alkali resistance is >3563h, and the salt resistance of Example 7 is >3596h, the acid resistance is >3204h, and the alkali resistance is >3285h. It can be seen that the corrosion resistance of Examples 12-14 is better than that of Example 7. The analysis is as follows: The difference between Examples 12-14 and Example 7 is that the silanization of silica causes the polar hydroxyl groups on the surface of silica to be replaced by non-polar methyl groups, so that the hydrophobicity of silica is improved, thereby improving the corrosion resistance of the corrosion-resistant coating, and then improving the corrosion resistance of the steel pipe body.

[0064] Specifically combining the test results of Example 3 and Comparative Example 1, the salt resistance of Example 3 is >2519h, the acid resistance is >2014h, and the alkali resistance is >2188h, while the salt resistance of Comparative Example 1 is >1524h, the acid resistance is >1032h, and the alkali resistance is >1185h. It can be seen that the corrosion resistance of Example 3 is better than that of Comparative Example 1. The analysis is as follows: The difference between Example 3 and Comparative Example 1 is that the network structure formed after the epoxy resin is cured is filled with graphite phase carbon nitride, thereby prolonging the penetration process of the corrosive electrolyte in the coating, so as to play a corrosion-resistant role through the barrier properties of the coating itself, thereby improving the corrosion resistance of the steel pipe body.

[0065] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A corrosion-resistant seamless steel pipe, comprising a steel pipe body (1), characterized in that: The surface of the steel pipe body (1) is provided with a corrosion-resistant coating (2), wherein the corrosion-resistant coating (2) is obtained by applying a corrosion-resistant coating to the surface of the steel pipe body (1), wherein the corrosion-resistant coating comprises the following components in percentage by mass: 55-60% epoxy resin, 13-17% graphite carbon nitride, 0.8-1.2% additive, and the remainder is filled with butyl acetate up to 100%.

2. The corrosion-resistant seamless steel pipe according to claim 1, characterized in that: The graphite phase carbon nitride is prepared by the following steps: The graphite phase carbon nitride, silicon dioxide and ethanol are mixed and stirred evenly, and then ethanol, deionized water and ammonia water are added, heated and stirred evenly, and then filtered, washed and dried to obtain modified graphite phase carbon nitride.

3. The corrosion-resistant seamless steel pipe according to claim 2, characterized in that: Benzotriazole is also added in the modification process of the graphite phase carbon nitride, that is, the modification preparation steps of the graphite phase carbon nitride are as follows: S100, mixing graphite phase carbon nitride, silicon dioxide and ethanol, stirring evenly, then adding ethanol, deionized water and ammonia water, heating and stirring evenly, filtering, washing and drying to obtain primary modified graphite phase carbon nitride; S200, adding primary modified graphite phase carbon nitride into an aqueous solution of tris(hydroxymethyl)aminomethane hydrochloride; Then, benzotriazepine dissolved in anhydrous ethanol is added, and finally a binder is added. After stirring evenly, the mixture is centrifuged and dried to obtain modified graphite phase carbon nitride.

4. The corrosion-resistant seamless steel pipe according to claim 3, characterized in that: The mass ratio of the graphite phase carbon nitride, silicon dioxide and benzotriazole is 0.1:(3.2-3.6):(2.1-2.5).

5. The corrosion-resistant seamless steel pipe according to claim 3, characterized in that: The binder is dopamine.

6. The corrosion-resistant seamless steel pipe according to claim 2, characterized in that: The silicon dioxide is prepared by the following steps: Silicon dioxide is added to anhydrous ethanol, and after ultrasonic treatment, trimethylchlorosilane is added, and after heating reaction, centrifugation is performed, and then the product is washed, dried, and ground to obtain modified silicon dioxide.

7. The corrosion-resistant seamless steel pipe according to claim 6, characterized in that: The mass ratio of silicon dioxide to trimethylchlorosilane is 1:(0.17-0.21).

8. The corrosion-resistant seamless steel pipe according to claim 1, characterized in that: The epoxy resin is bisphenol A type epoxy resin.

9. The corrosion-resistant seamless steel pipe according to claim 1, characterized in that: The auxiliary agent is formed by mixing organic silicon, polythiol and polyamide.

10. A method for preparing a corrosion-resistant seamless steel pipe according to claim 1, characterized in that: The steps include: S1. Mix graphite phase carbon nitride and butyl acetate and stir evenly, then add epoxy resin and additives, stir evenly, and let stand to prepare a corrosion-resistant coating; S2. Apply the corrosion-resistant coating to the surface of the steel pipe body, and after curing, obtain a corrosion-resistant seamless steel pipe.

Citation Information

Patent Citations

  • Silicon dioxide surface grafting modification method

    CN104312215A

  • Machining process capable of improving corrosion resistance of plastic-coated steel tube

    CN109321093A

  • Graphite phase like carbonitride / epoxy resin anti-corrosive coating, and preparation method and applications thereof

    CN110157296A

  • Nano silicon dioxide loaded graphite-like phase carbon nitride and preparation method thereof, and self-lubricating phenolic aldehyde laminated cloth bearing material and preparation method thereof

    CN114854230A

  • Corrosion-resistant low-alloy seamless steel tube and preparation method thereof

    CN115386793A

Cited By

  • Composite anti-icing coating with high hydrophobicity

    CN120137473A

  • Seamless steel tube for oil pipeline and preparation method of seamless steel tube

    CN120310371A