Modified manganese dioxide, preparation method and application

The K+-doped δ-MnO2 adsorption material was prepared by the hydrothermal method, which improved the oxidation adsorption capacity and adsorption efficiency of manganese dioxide, solved the problem of low adsorption efficiency of thallium ions by existing manganese dioxide, and achieved efficient thallium Ion removal effect.

CN118754204APending Publication Date: 2024-10-11CENT SOUTH UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410198596.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The adsorption efficiency of existing manganese dioxide for thallium ions is not high, making it difficult to effectively remove thallium ions in thallium-containing wastewater.

Method used

The δ-MnO2 adsorption material with a specific proportion of K+ doping is prepared by hydrothermal method to improve its oxidation adsorption capacity and adsorption efficiency, enhance the surface defects and vacancy ratio of the material, and improve the exchange adsorption capacity of thallium ions.

Benefits of technology

In a high-concentration thallium environment, the adsorption capacity is significantly improved, ensuring stable precipitation and efficient removal of thallium ions, and solving the problems of low efficiency and insufficient selectivity of existing thallium removal agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754204A_ABST
    Figure CN118754204A_ABST
Patent Text Reader

Abstract

The invention provides modified manganese dioxide as well as a preparation method and application thereof. The preparation method of the modified manganese dioxide comprises the following steps: S1, obtaining a mixed solution containing potassium permanganate, a reducing agent and potassium hydroxide; the molar ratio of potassium hydroxide to potassium permanganate is (1-3): 1; s2, carrying out hydrothermal treatment on the mixed solution to obtain a reaction solution containing the modified manganese dioxide; the temperature of the hydrothermal treatment is 80-140 DEG C, and the reaction time is 6-25 hours. The manganese dioxide is modified, so that the oxidation adsorption capacity and adsorption efficiency of the manganese dioxide on thallium are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of preparation of new materials and treatment of thallium-containing wastewater, and in particular relates to modified manganese dioxide, a preparation method and application. Background Art

[0002] Thallium is extremely toxic, even more so than other metals such as lead, cadmium and mercury. The lethal dose for adults is 10-15 mg / kg. Acute poisoning caused by it can lead to gastrointestinal damage, nerve paralysis and often hair loss symptoms. Thallium is widely used in high-tech industries, such as oxidants in organic synthesis, ceramic semiconductors, infrared spectrophotometers, alloys, electronic equipment, etc. The large-scale use of thallium causes thallium to continuously enter the external environment medium, seriously affecting human health and living environment, so achieving efficient thallium removal from wastewater has great practical significance. At present, the main methods for removing thallium from water bodies are chemical precipitation, biological method and activated carbon adsorption method. However, these methods often have problems such as large dosage, difficulty in meeting removal standards and secondary pollution due to the low thallium content in thallium-containing wastewater. Adsorption method is considered to be the most promising method for removing thallium from wastewater due to its easy recovery, high efficiency and wide adaptability.

[0003] Manganese dioxide (MnO2) can be used to adsorb thallium ions because of its abundant manganese-oxygen vacancies, defects and other adsorption active sites on its surface. In "Study on the Use of δ-MnO2 Materials for Removing Thallium from Wastewater and Its Thallium Removal Mechanism", Li Jinglong used a one-pot hydrothermal method to adjust different temperatures to prepare δ-MnO2 with different AOS. The oxidation ability of δ-MnO2 was used to oxidize Tl(Ⅰ) to Tl(Ⅲ) and precipitate on the surface of δ-MnO2; however, due to the limitation of interlayer ion capacity, not enough thallium ions can enter the interlayer and precipitate on the surface of the material, thus reducing the adsorption efficiency of thallium ions.

[0004] In view of this, it is necessary to provide a modified manganese dioxide, a preparation method and an application to solve or alleviate the technical defect that the existing manganese dioxide has low adsorption efficiency for thallium ions. Summary of the invention

[0005] The main purpose of the present invention is to provide a modified manganese dioxide, a preparation method and an application, aiming to solve or alleviate the technical problem that the existing manganese dioxide has low adsorption efficiency for thallium ions.

[0006] To achieve the above object, the present invention provides a method for preparing modified manganese dioxide, comprising the steps of:

[0007] S1, obtaining a mixed solution containing potassium permanganate, a reducing agent and potassium hydroxide;

[0008] The molar ratio of the potassium hydroxide to the potassium permanganate is 1 to 3:1;

[0009] S2, performing hydrothermal treatment on the mixed solution to obtain a reaction solution containing the modified manganese dioxide;

[0010] The temperature of the hydrothermal treatment is 80-140° C., and the reaction time is 6-25 hours.

[0011] Furthermore, the method for obtaining the mixed solution includes the following sub-steps:

[0012] S11, providing a potassium hydroxide solution, wherein the concentration of the potassium hydroxide solution is 0.01 to 0.05 g / mL;

[0013] S12, mixing the potassium permanganate and the reducing agent into the potassium hydroxide solution to obtain the mixed solution.

[0014] Furthermore, the reducing agent includes one or more of ammonium oxalate, manganese sulfate, hydrochloric acid, and sulfuric acid.

[0015] Furthermore, the molar ratio of the potassium hydroxide to the potassium permanganate is 2-3:1; and / or the molar ratio of the potassium permanganate to the reducing agent is 1:0.5-1.

[0016] Furthermore, the step S2 further comprises: performing solid-liquid separation on the reaction liquid to obtain the modified manganese dioxide.

[0017] Furthermore, the step S2 further comprises: drying and grinding the modified manganese dioxide in sequence to obtain the modified manganese dioxide in powder form.

[0018] Furthermore, the drying temperature is 60 to 90° C., and the drying time is 10 to 15 hours.

[0019] The present invention also provides a modified manganese dioxide, which is prepared by any of the above-mentioned preparation methods.

[0020] The present invention also provides a use of any of the modified manganese dioxide described above in removing thallium.

[0021] The present invention also provides a method for removing thallium, comprising: adding any of the modified manganese dioxide described above into thallium-containing wastewater, wherein the pH of the thallium-containing wastewater is 2-4 or 7-9.

[0022] Compared with the prior art, the present invention has at least the following advantages:

[0023] The present invention uses a hydrothermal method to prepare a product having a specific ratio of K +The doped δ-MnO2 adsorption material improves the oxidation adsorption capacity and adsorption efficiency of manganese dioxide for thallium; in a high concentration of thallium environment, the adsorption capacity is excellent and it is not easy to desorb, thus solving the problems of low thallium removal efficiency and weak selectivity of existing thallium removal adsorbents. Specifically, in the initial stage of material synthesis, the present invention can control the degree of K embedding of δ-MnO2 and the characterization of the product by combining KOH and potassium permanganate in a specific ratio; and because K + The embedding of Tl increases the surface defects and vacancy ratio of MnO2, and the AOS, that is, the oxidation ability, also changes, making the prepared MnO2 have excellent ion exchange adsorption ability; at the same time, due to the increase in active sites, Tl can form a stable complex and precipitate on the surface of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0025] Figure 1 The SEM images of K / Mn=0 before and after absorbing thallium in the present invention; wherein, (a)-1 is a SEM image of K / Mn=0 magnified 20,000 times, and (a)-2 is a SEM image of K / Mn=0 after absorbing thallium magnified 20,000 times;

[0026] Figure 2 The SEM images of K / Mn=0.4 before and after absorbing thallium in the present invention; wherein, (b)-1 is a SEM image of K / Mn=0.4 magnified 20,000 times, and (b)-2 is a SEM image of K / Mn=0.4 after absorbing thallium magnified 20,000 times;

[0027] Figure 3 The SEM images of K / Mn=0.8 before and after absorbing thallium in the present invention; wherein, (c)-1 is a SEM image of K / Mn=0.8 magnified 20,000 times, and (c)-2 is a SEM image of K / Mn=0.8 after absorbing thallium magnified 20,000 times;

[0028] Figure 4 The SEM images of K / Mn=2.5 before and after absorbing thallium in the present invention; wherein, (d)-1 is a SEM image of K / Mn=2.5 magnified 20,000 times, and (d)-2 is a SEM image of K / Mn=2.5 after absorbing thallium magnified 19,000 times;

[0029] Figure 5The XRD patterns of the products prepared in Example 1 and Comparative Examples 1-3 of the present invention are as follows;

[0030] Figure 6 The thallium removal effect diagram of the products prepared in Example 1 and Comparative Examples 1-3 of the present invention.

[0031] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0034] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0035] The present invention provides a method for preparing modified manganese dioxide, comprising the steps of:

[0036] S1, obtaining a mixed solution containing potassium permanganate, a reducing agent and potassium hydroxide.

[0037] The present invention can increase the K ion content between MnO2 layers by using the potassium permanganate, the reducing agent and the potassium hydroxide as reactants.

[0038] The molar ratio of potassium hydroxide to potassium permanganate is 1 to 3:1; preferably, the molar ratio of potassium hydroxide to potassium permanganate is 2 to 3:1. By limiting the ratio of potassium hydroxide to potassium permanganate, a specific potassium-doped manganese dioxide material with high efficiency in removing thallium can be obtained, and it has the following characteristics: Figure 4 and Figure 5 Characterization shown in .

[0039] The molar ratio of the potassium permanganate to the reducing agent is 1:0.5-1; by limiting the ratio of the potassium permanganate to the reducing agent, the target crystal form of MnO2 can be effectively prepared.

[0040] The reducing agent may include one or more of ammonium oxalate, manganese sulfate, concentrated hydrochloric acid, and concentrated sulfuric acid; further, it may be ammonium oxalate; by limiting the type of the reducing agent, the success rate of preparing the target modified MnO2 can be improved.

[0041] In the present invention, the method for obtaining the mixed solution may include the following sub-steps:

[0042] S11, providing a potassium hydroxide solution, wherein the concentration of the potassium hydroxide solution is 0.01 to 0.05 g / mL.

[0043] S12, mixing the potassium permanganate and the reducing agent into the potassium hydroxide solution to obtain the mixed solution.

[0044] The process of mixing the potassium permanganate and the reducing agent into the potassium hydroxide solution may include: adding the potassium permanganate and the reducing agent into the potassium hydroxide solution, and then mixing for 20 to 60 minutes.

[0045] S2, performing hydrothermal treatment on the mixed solution to obtain a reaction solution containing the modified manganese dioxide.

[0046] In the present invention, the temperature of the hydrothermal treatment is 80-140°C or 90-140°C or 90-100°C, and the reaction time is 6-25h; by limiting the temperature and duration of the hydrothermal treatment, the desired modified MnO2 can be obtained within limited time and energy requirements, which is beneficial to practical applications.

[0047] In the present invention, after obtaining the reaction liquid, in order to further obtain the modified manganese dioxide, the reaction liquid can also be subjected to solid-liquid separation treatment to obtain the modified manganese dioxide; then, the modified manganese dioxide is sequentially dried and ground to obtain the powdered modified manganese dioxide, and the powdered modified manganese dioxide can pass through a 200-mesh sieve; the drying temperature can be 60 to 90° C., and the drying time can be 10 to 15 hours.

[0048] The present invention also provides a modified manganese dioxide, which is prepared by any of the above-mentioned preparation methods. Specifically, the modified manganese dioxide may contain 33-39% oxygen, 12-14% potassium, and 47-55% manganese by weight.

[0049] The present invention also provides a use of any of the modified manganese dioxide described above in removing thallium.

[0050] The present invention also provides a thallium removal method, comprising: adding any of the modified manganese dioxide described above into thallium-containing wastewater and mixing; the mixing time can be 0.5 to 2 hours, and the rotation speed can be 300 to 400 r / min; the thallium-containing wastewater can include one or more of TlNO3 and Tl(NO3)3, the pH of the thallium-containing wastewater is 2 to 4 or 7 to 9, and the thallium-containing wastewater can contain one or more of monovalent thallium ions and trivalent thallium ions; the concentration of thallium ions in the thallium-containing wastewater can be 18 to 100 ppm.

[0051] It should be noted that although Liu Juchao used α-MnO2 and δ-MnO2 as adsorbents to add to thallium-containing wastewater in Effects of MnO2 crystal structure on the sorption and oxidative reactivity toward thallium(I) in the α-MnO2 pore structure, the K + The content is far less than that of δ-MnO2, and ordinary δ-MnO2 lacks K in the synthesis process. + The present invention is aimed at the ion exchange-oxidation mechanism of manganese dioxide to remove Tl, and K + By doping, MnO2 with different proportions between crystal planes is obtained, thereby obtaining a MnO2 adsorbent with different manganese oxygen vacancies, active sites and oxidation precipitation capabilities.

[0052] Specifically, the present invention adds potassium permanganate and a reducing agent to the KOH solution, stirs it thoroughly, and then prepares potassium-doped δ-MnO2 through a hydrothermal reaction; then the potassium-doped δ-MnO2 is used as an adsorbent and put into thallium-containing simulated wastewater for adsorption reaction to achieve efficient thallium removal. Since potassium ions are pre-embedded between the δ-MnO2 layers, the layered structure of the crystal contains more K + More stable; and using the similarity of K-Tl, during the reaction, Tl + Can enter the interlayer and K + exchange, thus achieving efficient and stable thallium removal.

[0053] The following are specific examples of the present invention:

[0054] Example 1

[0055] Dissolve 2.805 g KOH in 70 mL deionized water, stir magnetically to obtain a potassium hydroxide solution; add 3.1606 g KMnO4 and 1.4211 g (NH4)2C2O4 to the potassium hydroxide solution, stir for 30 min, and obtain a mixed solution.

[0056] The mixed solution was transferred to a 100 mL polytetrafluoroethylene autoclave and maintained at 90° C. for 24 h to obtain a reaction solution. After the reaction solution was cooled to room temperature, it was washed alternately with anhydrous ethanol and deionized water for 3 times and the solid product was separated by suction filtration. The solid product was placed in an oven at 80° C. and dried for 12 h, then ground into powder, passed through a 200-mesh sieve, and the material under the sieve was taken as the prepared product, named K / Mn=2.5.

[0057] Comparative Example 1

[0058] Compared with Example 1, in this comparative example, 2.805 g of KOH was adjusted to 0 g of KOH (ie, the potassium hydroxide solution was replaced with 70 mL of deionized water), and other conditions remained unchanged; the prepared product in this comparative example was named K / Mn=0.

[0059] Comparative Example 2

[0060] Compared with Example 1, in this comparative example, 2.805 g of KOH was adjusted to 0.448 g of KOH, and other conditions remained unchanged; the prepared product in this comparative example was named K / Mn=0.4.

[0061] Comparative Example 3

[0062] Compared with Example 1, in this comparative example, 2.805 g of KOH was adjusted to 0.897 g of KOH, and other conditions remained unchanged; the prepared product in this comparative example was named K / Mn=0.8.

[0063] Analysis example 1

[0064] 1. The SEM images of the products prepared in Example 1 and Comparative Examples 1-3 are as follows: Figure 1-4 As shown, it can be seen that the surface defect and vacancy ratio of K / Mn=2.5 is increased, and it has pores and a larger specific surface area.

[0065] 2. XRD characterization of the products prepared in Example 1 and Comparative Examples 1-3 is as follows: Figure 5 As shown, compared with the standard card PDF#86-0666, it can be seen that: the position of its diffraction peak is completely consistent with the position of the diffraction peak of the standard card and there are no other impurity peaks. The four peaks correspond to the (003), (006), (012), and (113) crystal planes respectively, confirming that the prepared material is δ-MnO2.

[0066] 3. The elemental analysis of the products prepared in Example 1 and Comparative Examples 1-3 is shown in the following table. It can be seen that MnO2 with different K contents can be obtained by changing the ratio of potassium hydroxide to potassium permanganate.

[0067]

[0068]

[0069] 4. The prepared products in Example 1 and Comparative Examples 1-3 were respectively used as test materials to carry out thallium adsorption tests. The specific test process is as follows:

[0070] At room temperature, 10 mg of the material to be tested was added to 125 mL of thallium-containing simulated wastewater and stirred for 120 minutes to remove thallium from the thallium-containing simulated wastewater; wherein the thallium ion concentration in the thallium-containing simulated wastewater (TlNO3 solution) was 20 ppm (mg / L), and the pH of the thallium-containing simulated wastewater was 2.

[0071] See also Figure 1-4 As shown in Figure 3, the adsorbed MnO2 particles are larger, indicating the precipitation adsorption of Tl on the surface.

[0072] See also Figure 6 As shown, the test results are: the total thallium removal rates corresponding to K / Mn=0, K / Mn=0.4, K / Mn=0.8, and K / Mn=2.5 are 90.76%, 88.71%, 81.27%, and 97.85%, respectively.

[0073] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing modified manganese dioxide, characterized in that: Includes steps: S1, obtaining a mixed solution containing potassium permanganate, a reducing agent and potassium hydroxide; The molar ratio of the potassium hydroxide to the potassium permanganate is 1 to 3:1; S2, performing hydrothermal treatment on the mixed solution to obtain a reaction solution containing the modified manganese dioxide; The temperature of the hydrothermal treatment is 80-140° C., and the reaction time is 6-25 hours.

2. The preparation method according to claim 1, characterized in that: The method for obtaining the mixed solution comprises the following sub-steps: S11, providing a potassium hydroxide solution, wherein the concentration of the potassium hydroxide solution is 0.01 to 0.05 g / mL; S12, mixing the potassium permanganate and the reducing agent into the potassium hydroxide solution to obtain the mixed solution.

3. The preparation method according to claim 1, characterized in that: The reducing agent includes one or more of ammonium oxalate, manganese sulfate, hydrochloric acid, and sulfuric acid.

4. The preparation method according to claim 1, characterized in that: The molar ratio of the potassium hydroxide to the potassium permanganate is 2-3:1; and / or the molar ratio of the potassium permanganate to the reducing agent is 1:0.5-1.

5. The preparation method according to claim 1, characterized in that: The step S2 further comprises: performing solid-liquid separation on the reaction liquid to obtain the modified manganese dioxide.

6. The preparation method according to claim 5, characterized in that: The step S2 further comprises: drying and grinding the modified manganese dioxide in sequence to obtain the modified manganese dioxide in powder form.

7. The preparation method according to claim 6, characterized in that: The drying temperature is 60-90° C., and the drying time is 10-15 hours.

8. A modified manganese dioxide, characterized in that The preparation is carried out by the preparation method according to any one of claims 1 to 7.

9. Use of the modified manganese dioxide as claimed in claim 8 in removing thallium.

10. A method for removing thallium, characterized in that: include: The modified manganese dioxide as claimed in claim 8 is added to thallium-containing wastewater, wherein the pH of the thallium-containing wastewater is 2-4 or 7-9.

Citation Information

Cited By

  • Fluorine-doped alpha-phase manganese dioxide nanotube, preparation method thereof and application of nanotube as thallium adsorption material

    CN121155509A