Spinel glass ceramic and application thereof

By optimizing the composition and crystal phase structure of spinel glass ceramics, chemical strengthening is achieved, which solves the problem of insufficient drop resistance and extrusion resistance of existing glass products and improves mechanical strength and damage resistance.

CN118754445AActive Publication Date: 2024-10-11CHONGQING AUREAVIA HI TECH GLASS CO LTD

Patent Information

Application Number
CN202410741381.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-25
Filing Date
2024-06-07
Publication Date
2024-10-11
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing glass products are easily broken when dropped, squeezed or impacted, and it is difficult to achieve high compressive stress layer depth and deep stress, which affects their anti-drop and anti-extrusion properties.

Method used

By optimizing the composition and crystal phase structure of spinel glass ceramics, including the mole percentages of SiO2, Al2O3, ZrO2, MgO, ZnO, Na2O and Li2O, adding (Zn, Mg)Al2O4 and tetragonal ZrO2 crystal phases, the crystal phase content and Crystal size, chemical strengthening is achieved to obtain ultra-high compressive stress layer depth and deep stress.

Benefits of technology

The mechanical strength and damage resistance of spinel glass ceramics are significantly improved, especially the drop impact resistance and extrusion resistance, ensuring that it has high mechanical strength and excellent light transmittance after chemical strengthening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754445A_ABST
    Figure CN118754445A_ABST
Patent Text Reader

Abstract

According to the spinel glass ceramic and the application thereof provided by the invention, the spinel glass ceramic has a specific composition and a crystal phase structure, so that not only is the spinel glass ceramic endowed with high intrinsic strength, but also the spinel glass ceramic can obtain an expected stress structure after chemical strengthening treatment; particularly, the depth of an ultra-high compression stress layer and the large deep layer stress are achieved. The reinforced spinel glass ceramic with high mechanical strength and damage resistance can be prepared by using the spinel glass ceramic.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application claims the priority of the Chinese patent application filed with the State Intellectual Property Office of China on December 25, 2023, with application number 2023118027864 and invention name “A spinel glass ceramic and its application”, the entire contents of which are incorporated by reference into this application. Technical Field

[0002] The present application relates to the technical field of glass ceramics, and in particular to a spinel glass ceramic and applications thereof. Background Art

[0003] Common situations in which protective glass for electronic equipment breaks include falling and breaking, crushing and breaking due to contact with other objects, or impact crushing caused by heavy objects falling and colliding. Analyzing the process of falling and breaking, it is roughly due to the collision of the glass surface with sharp objects (such as fine sand, cement, pebbles) with equal or greater hardness, resulting in local damage, forming a hemispherical crack extension source at the point of damage, partially attenuating the collision energy, and further expanding the remaining energy. When the compressive stress level on the glass surface is not enough to offset the remaining energy, the crack extension will pass through the glass surface area. When the longitudinal crack passes through the depth of the compressive stress layer to reach the tensile stress layer (or also called the tensile stress layer) area, the crack will quickly expand in the tensile stress area, causing the crack to penetrate the entire glass, thereby causing the glass to break or fracture. Analyzing the process of crushing or impact crushing, it is mainly because the force of the crushing or collision is greater than the surface compressive stress level of the glass, resulting in the glass being unable to offset the energy of the crushing impact.

[0004] It can be seen that the surface stress level, depth of the compressive stress layer and deep stress of glass products are closely related to their resistance to drop damage, extrusion damage and impact damage. When the depth of the compressive stress layer is constant, the greater the deep stress, the more residual energy of drop collision, extrusion or impact that can be offset by the surface compressive stress level. When the surface compressive stress level is not enough to offset the residual energy of drop collision, extrusion or impact, the deeper the depth of the compressive stress layer of the glass, the more conducive it is to offset the energy that drives the crack to expand.

[0005] Therefore, in order to further improve the drop impact resistance and extrusion resistance of glass-ceramics with spinel as the main crystal phase, it is necessary to develop a spinel glass-ceramic that can obtain a larger deep stress and an ultra-high compressive stress layer depth through chemical strengthening, and use the spinel glass-ceramic to prepare reinforced glass-ceramics with high mechanical strength. Summary of the invention

[0006] The purpose of the present application is to provide a spinel glass-ceramic and its application. The spinel glass-ceramic can be obtained by chemical strengthening to obtain a reinforced spinel glass-ceramic with large deep stress and ultra-high compressive stress layer depth, thereby improving the mechanical strength and damage resistance of the reinforced spinel glass-ceramic, especially improving its drop impact resistance and extrusion resistance.

[0007] The technical solutions provided by this application are as follows:

[0008] In a first aspect, a spinel glass ceramic is provided, wherein the composition of the spinel glass ceramic comprises, in terms of molar percentage of oxides: SiO2 35.00mol% to 60.00mol%, Al2O3 20.00mol% to 40.00mol%, ZrO2 2.00mol% to 8.00mol%, MgO 3.00mol% to 7.50mol%, ZnO 7.00mol% to 13.00mol%, Na2O 1.00mol% to 10.00mol%, and Li2O 2.50mol% to 10.00mol%;

[0009] The spinel glass ceramic contains 15.00 wt % to 45.00 wt % of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramic;

[0010] Take W [(Zn,Mg)Al2O4] is the weight percentage of (Zn, Mg)Al2O4 phase in the spinel glass ceramic, W [Al2O3] is the weight percentage of Al2O3 in the spinel glass ceramic, W [MgO] is the weight percentage of MgO in the spinel glass ceramic, W [ZnO] is the weight percentage of ZnO in the spinel glass ceramic;

[0011] A=(1-W [(Zn,Mg)Al2O4] / 2)×W [Al2O3] / 2,

[0012] B=(1-W [(Zn,Mg)Al2O4] )×(W [MgO] +W [ZnO] ),

[0013] C=A / B, in the spinel glass-ceramics, 1.50≤C≤1.85.

[0014] The spinel glass ceramics of the present application have a specific composition and crystal phase structure. The synergistic effect of the composition and crystal phase structure not only gives the spinel glass ceramics high intrinsic strength, but also ensures that the spinel glass ceramics obtain the desired stress structure after chemical strengthening treatment, especially ultra-high compressive stress layer depth and large deep stress. The spinel glass ceramics can be used to prepare reinforced spinel glass ceramics with high mechanical strength and high damage resistance.

[0015] In some embodiments of the present application, in the spinel glass ceramic, the value of A is 10.00% to 25.00%, preferably 14.00% to 25.00%; and / or the value of B is 7.50% to 12.50%, preferably 8.00% to 12.00%. By making the values ​​of A and B meet the above ranges, it is helpful to make the composition and structure of the spinel glass ceramic meet the value range of C.

[0016] In some embodiments of the present application, the spinel glass ceramic further comprises a tetragonal ZrO2 crystal phase, and the total content of the (Zn, Mg)Al2O4 crystal phase and the tetragonal ZrO2 crystal phase accounts for 25.00 wt% to 70.00 wt% of the spinel glass ceramic, preferably 30.00 wt% to 50.00 wt% of the spinel glass ceramic. When the total crystal phase content W of the (Zn, Mg)Al2O4 crystal phase and the tetragonal ZrO2 crystal phase in the spinel glass ceramic is within the above range, it can ensure that the spinel glass ceramic has a large number of crystals that can hinder crack propagation, which is beneficial to improve the intrinsic strength or inherent strength of the spinel glass ceramic.

[0017] In some embodiments of the present application, in the spinel glass ceramics, the ratio of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase is 1.00 to 18.00, preferably 1.00 to 15.00. When the ratio of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase in the spinel glass ceramics (i.e., the mass ratio Z of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase) is within the above range, the spinel glass ceramics can be endowed with a specific crystal phase structure, which is not only conducive to improving the intrinsic strength or inherent strength of the spinel glass ceramics, but also conducive to enabling the spinel glass ceramics to obtain a desired stress structure during chemical strengthening.

[0018] In some embodiments of the present application, in the spinel glass ceramics, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is 3.0nm to 10.0nm, preferably 4.0nm to 8.0nm, more preferably 4.0nm to 7.5nm, and further preferably 4.5nm to 7.5nm. When the average crystal size of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramics is within the above range, it not only helps to improve the light transmittance of the spinel glass ceramics while ensuring the strength of the spinel glass ceramics, but also helps to improve the ion exchange performance of the spinel glass ceramics, so that it can obtain the desired stress level through chemical strengthening.

[0019] In some embodiments of the present application, the composition of the spinel glass ceramics further comprises, in terms of molar percentage of oxides: K2O 0.00mol% to 5.00mol%, CaO 0.00mol% to 10.00mol%, B2O3 0.00mol% to 10.00mol%, BaO 0.00mol% to 5.00mol%. In the glass system of the present application, K2O, CaO, B2O3 or BaO as optional components, the appropriate amount of which can improve the forming effect, crystallization effect, chemical strengthening effect or optical effect of the spinel glass ceramics.

[0020] In some embodiments of the present application, the composition of the spinel glass ceramics includes, in terms of molar percentage of oxides: SiO2 35.00mol% to 60.00mol%, Al2O3 20.00mol% to 40.00mol%, ZrO2 2.00mol% to 8.00mol%, MgO 4.00mol% to 7.00mol%, ZnO 9.00mol% to 12.00mol%, Na2O 2.00mol% to 10.00mol%, Li2O 3.00mol% to 10.00mol%. By properly adjusting the content of MgO, ZnO, Li2O or Na2O, it is helpful to ensure that the main crystalline phase content in the spinel glass ceramics meets the desired level, and it is also helpful to ensure that the spinel glass ceramics achieve the desired chemical strengthening effect, thereby obtaining a strengthened spinel glass ceramic with a high stress level.

[0021] In some embodiments of the present application, the composition of the spinel glass ceramics includes, in terms of the molar percentage of oxides: SiO2 35.00mol% to 50.00mol%, Al2O3 25.00mol% to 35.00mol%, ZrO23.00mol% to 5.00mol%, MgO 4.00mol% to 7.00mol%, ZnO 9.00mol% to 12.00mol%, Na2O2.00mol% to 10.00mol%, Li2O3.00mol% to 10.00mol%. By properly adjusting the content of each necessary oxide, it is helpful to ensure that the spinel glass ceramics achieve the desired crystalline phase structure and glass network structure that can achieve a high stress level, thereby facilitating the acquisition of a strengthened spinel glass ceramic with a high stress level.

[0022] In some embodiments of the present application, the composition of the spinel glass ceramics satisfies, based on the molar percentage of each oxide in the spinel glass ceramic composition:

[0023] 1.30≤ZnO / MgO≤2.50; and / or,

[0024] 0.05≤Li2O / (Al2O3-(MgO+ZnO)+SiO2)≤0.20; and / or,

[0025] 0.19≤(Al2O3-(MgO+ZnO)) / SiO2≤0.60; and / or,

[0026] 0.26≤Na2O / Li2O≤3.00.

[0027] By making the spinel glass ceramics of the present application satisfy at least one of the above-mentioned relationships ZnO / MgO, Li2O / (Al2O3-(MgO+ZnO)+SiO2), (Al2O3-(MgO+ZnO)) / SiO2, and Na2O / Li2O, it helps to further adjust the network structure and crystal phase structure of the spinel glass ceramics, so that the spinel glass ceramics form a specific microstructure that helps to obtain the desired stress level.

[0028] In some embodiments of the present application, the composition of the spinel glass ceramics further satisfies the following conditions, based on the molar percentage of each oxide in the spinel glass ceramic composition:

[0029] 12.00mol%≤ZnO+MgO≤20.00mol%, preferably, 13.00mol%≤ZnO+MgO≤17.30mol%; and / or,

[0030] 9.00mol%≤Al2O3-(MgO+ZnO)≤22.00mol%, preferably, 10.00mol%≤Al2O3-(MgO+ZnO)≤20.00mol%; and / or,

[0031] 5.00 mol%≤Na2O+Li2O≤15.00 mol%, preferably, 6.00 mol%≤Na2O+Li2O≤13.50 mol%.

[0032] The spinel glass ceramics of the present application satisfy at least one of the above-mentioned relationships ZnO+MgO, Al2O3-(MgO+ZnO), and Na2O+Li2O, which helps to obtain a high content of (Zn, Mg)Al2O4 crystal phase with high hardness and high modulus to further improve the intrinsic strength or inherent strength of the spinel glass ceramics, or, helps to further improve the ion exchange effect of the spinel glass ceramics to obtain the desired stress level.

[0033] In some embodiments of the present application, the spinel glass-ceramic is transparent in the visible light range.

[0034] In some embodiments of the present application, the transmittance of the 0.7 mm thick spinel glass ceramic at 550 nm wavelength light is greater than or equal to 85%. The transmittance of the 0.7 mm thick spinel glass ceramic at 550 nm wavelength light is within the above range, indicating that the spinel glass ceramic of the present application has high light transmittance. At the same time, the spinel glass ceramic of the present application can also obtain high mechanical strength and high damage resistance through chemical strengthening treatment, which effectively broadens the application scenarios and application fields of the spinel glass ceramic of the present application.

[0035] By making the spinel glass ceramics meet a specific crystal phase structure, on the one hand, it is beneficial for the spinel glass ceramics to obtain high intrinsic strength, and on the other hand, it is beneficial to improve the chemical strengthening effect of the spinel glass ceramics, so that it can obtain ultra-high compressive stress layer depth and large deep stress through chemical strengthening, which is beneficial to improve the mechanical strength and damage resistance of the spinel glass ceramics. The relevant characteristics of the X-ray diffraction spectrum can reflect the crystal phase structure of the glass ceramics, including crystal phase composition, crystal size, etc.

[0036] In some embodiments of the present application, in the X-ray diffraction spectrum of the spinel glass ceramic, the peak with the maximum peak intensity in the characteristic peak with a 2θ angle in the range of 28° to 32° is taken as the first characteristic peak, and the peak with the maximum peak intensity in the characteristic peak with a 2θ angle in the range of 36° to 38° is taken as the second characteristic peak, and the peak intensity ratio X of the first characteristic peak and the second characteristic peak is 0.80 to 1.50, preferably 0.85 to 1.30. The peak intensity ratio X of the spinel glass ceramic is within the above range, indicating that the spinel glass ceramic has obtained a suitable crystal integrity, which helps to ensure that the spinel glass ceramic obtains better optical effects and strengthening effects.

[0037] In some embodiments of the present application, in the X-ray diffraction pattern of the spinel glass-ceramic, the characteristic peak of the

[400] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 44° to 46°, the characteristic peak of the

[311] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 34° to 38°, and the characteristic peak of the

[440] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 64° to 67°;

[0038] The half-peak width W of the characteristic peak of the

[400] crystal plane is

[400] 0.650°~1.800°, preferably W

[400] 0.900° to 1.600°;

[0039] The half-peak width W of the characteristic peak of the

[311] crystal plane is

[311] 0.900°~2.800°, preferably W

[311] 1.100° to 2.230°;

[0040] The half-peak width W of the characteristic peak of the

[440] crystal plane is

[440] 0.750°~2.000°, preferably W

[440] The W of spinel glass ceramics is 0.900° to 1.600°.

[400] , W

[311] , W

[440] Within the above range, it is shown that the (Zn, Mg)Al2O4 crystal phase in the crystal phase structure of the spinel glass ceramic has a suitable average crystal size and satisfies a specific crystal phase structure, which is not only conducive to giving the spinel glass ceramic a high intrinsic strength or inherent strength, but also conducive to ensuring that the spinel glass ceramic obtains an ideal stress structure after chemical strengthening. At the same time, it is helpful for the spinel glass ceramic to obtain the desired optical properties.

[0041] In a second aspect, a glass device is provided, which is made of the spinel glass ceramic in any one of the aforementioned embodiments.

[0042] In a third aspect, an electronic device is provided, comprising the spinel glass ceramic according to any one of the aforementioned embodiments.

[0043] In some embodiments of the present application, the electronic device includes at least one of a mobile phone, a tablet computer, a smart wearable, a display, and a television.

[0044] One or more technical solutions of the present application have the following advantages or beneficial effects:

[0045] The present application provides a spinel glass ceramic with a specific composition and crystal phase structure. The synergistic effect of the composition and crystal phase structure not only gives the spinel glass ceramic a high intrinsic strength, but also ensures that the spinel glass ceramic obtains a desired stress structure after chemical strengthening treatment, especially an ultra-high compressive stress layer depth and a large deep stress. The spinel glass ceramic can be used to prepare a reinforced spinel glass ceramic with high mechanical strength and high damage resistance. Of course, it is not necessary to achieve all of the advantages described above at the same time to implement any product or method of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0047] Figure 1 Schematic diagram of the structure of the reinforced glass ceramic in the prior art, wherein t is the thickness of the glass, d is the depth of the compressive stress layer, 11 is the compressive stress layer, and 12 is the tensile stress layer;

[0048] Figure 2 It is a comparison diagram of the XRD diffraction patterns of the spinel glass ceramics in Examples 1 to 3 and Comparative Examples 6 to 9;

[0049] Figure 3 Schematic diagram of XRD diffraction curve fitting of spinel glass ceramics in Example 6;

[0050] Figure 4 is the XRD diffraction pattern of the spinel glass ceramic in Comparative Example 8;

[0051] Figure 5 is the XRD diffraction pattern of the spinel glass ceramic in Example 1;

[0052] Figure 6 is the XRD diffraction pattern of the spinel glass ceramic in Comparative Example 10;

[0053] Figure 7is the XRD diffraction pattern of the spinel glass ceramic in Comparative Example 11;

[0054] Figure 8 is the transmittance curve of the spinel glass ceramic in Example 1 under different wavelength conditions;

[0055] Fig. 9 The XRD diffraction comparison diagram of the spinel glass ceramic before and after chemical strengthening in Example 1;

[0056] Fig.10 It is a comparison diagram of the transmittance curves of the spinel glass ceramics before and after chemical strengthening under different wavelength conditions in Example 1;

[0057] Fig.11 is the XRD diffraction pattern of the spinel glass ceramic in Example 2;

[0058] Fig.12 A schematic diagram of the process of the single-rod static pressure strength test in this application;

[0059] Fig.13 This is a schematic diagram of the structure of the fixture for single-rod static pressure strength testing in this application;

[0060] Fig.14 This is a schematic diagram of the cross-sectional structure of the single-rod static pressure strength test fixture of the present application. DETAILED DESCRIPTION

[0061] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0062] Explanation of terms

[0063] DOL_0: Depth of compressive stress layer, also known as depth of compressive stress layer, refers to the distance along the thickness direction from any surface of strengthened glass ceramics (such as the strengthened spinel glass ceramics obtained by chemical strengthening treatment of spinel glass ceramics in this application) to the position where the compressive stress is zero near the surface.

[0064] |CT_AV|: refers to the absolute value of the average tensile stress in the tensile stress layer, specifically refers to the absolute value of the average value of all tensile stresses in the tensile stress layer.

[0065] CS_50: refers to the compressive stress value at a depth of 50μm from the surface of the strengthened glass-ceramic along the thickness direction.

[0066] |CT_CV|: refers to the absolute value of the maximum tensile stress in the tensile stress layer, specifically refers to the absolute value of the maximum value of all tensile stresses in the tensile stress layer.

[0067] Crystalline content: refers to the percentage of the mass of the crystal phase in the glass-ceramic to the total mass of the glass-ceramic.

[0068] Peak intensity: refers to the height of the diffraction peak in the XRD spectrum.

[0069] Half-peak width: refers to the width of the half-peak height of the diffraction peak in the XRD spectrum, usually expressed as an angle or 2θ value.

[0070] Substrate glass: refers to glass that has not been nucleated, crystallized or strengthened, or is also called basic glass.

[0071] Glass ceramics: also known as microcrystalline glass or crystallized glass, is a type of solid composite material that contains both a glass phase and a microcrystalline phase (or also called a crystal phase, a crystal phase, or a crystalline phase).

[0072] Theoretically, when the depths of the compressive stress layers extending inward from the two main surfaces of the glass product are equal or approximately equal, and the sum of the depths of the two compressive stress layers is equal to the thickness of the tensile stress layer, that is, Figure 1 As shown, the depth d of the compressive stress layer 11 on both sides is approximately equal to 25% of the thickness t of the glass 10, and the thickness of the tensile stress layer 12 is approximately equal to 50% of the thickness t of the glass 10, and the glass will reach the ideal compressive stress layer depth. However, in fact, in the prior art, almost no glass products have achieved the target effect of the compressive stress layer depth d being approximately equal to 25% of the glass thickness t. On the one hand, this compressive stress layer depth is relatively difficult to achieve. On the other hand, in the existing glass products, a higher compressive stress layer depth is often accompanied by a decrease in the surface stress level and a decrease in the overall strength of the glass products. Because in the ion exchange process of chemical strengthening treatment, the diffusion of ions becomes more difficult the deeper they go, and simply increasing the diffusion amount by adding alkali metal ions is very likely to cause bursting and fragmentation problems due to excessive internal stress before reaching a higher depth. In addition, for many glass products, after the exchange ion diffusion reaches a certain depth and the stress reaches a certain level, stress relaxation will occur, the depth will increase slightly or not increase, but the stress will decrease significantly, resulting in a decrease in the strength of the glass products. Therefore, at present, the only way to make the compressive stress depth of glass products as close to this ideal effect as possible. For spinel glass-ceramics containing the main crystalline phase as (Zn, Mg)Al2O4 crystalline phase (in this application, (Zn, Mg)Al2O4 is used to represent the solid solution of zinc spinel and magnesium spinel, or also called zinc aluminum spinel-magnesium aluminum spinel solid solution, zinc magnesium spinel solid solution, zinc spinel-magnesium spinel solid solution, zinc magnesium aluminum spinel solid solution), simply by increasing and introducing the absolute number and type of metal ions that can be ion-exchanged, it is not possible to ensure the realization of ultra-high stress layer depth and deep stress. On the one hand, when the Li inside the spinel glass-ceramics+ and Na + When the content exceeds a certain amount, it is easy to affect the network structure and crystal phase structure of the spinel glass ceramics, resulting in the problem of being unable to obtain the desired spinel glass ceramics; on the other hand, the stress distribution and stress effect that can be obtained after chemical strengthening of the glass ceramics are jointly affected by the composition and crystal phase structure of the glass ceramics. Simply increasing the absolute number and type of alkali metal ions that can be exchanged cannot guarantee that the spinel glass ceramics will obtain a crystal phase structure that can achieve the desired stress distribution.

[0073] Without being limited by theory, the composition and crystal phase structure of spinel glass-ceramics are closely related to the stress distribution or stress structure after chemical strengthening. By making the spinel glass-ceramics meet specific composition and crystal phase structure, the spinel glass-ceramics can be chemically strengthened to obtain strengthened spinel glass-ceramics with ultra-high compressive stress layer depth and large deep stress, thereby achieving high mechanical strength and high damage resistance of spinel glass-ceramics.

[0074] In view of this, a spinel glass ceramic having a specific composition and crystal phase structure and capable of obtaining a desired stress structure through chemical strengthening and its application are provided.

[0075] In some embodiments of the present application, a spinel glass ceramic is provided, and the composition of the spinel glass ceramic includes, in terms of molar percentage of oxides: SiO2 35.00mol% to 60.00mol%, Al2O3 20.00mol% to 40.00mol%, ZrO2 2.00mol% to 8.00mol%, MgO 3.00mol% to 7.50mol%, ZnO 7.00mol% to 13.00mol%, Na2O1.00mol% to 10.00mol%, Li2O 2.50mol% to 10.00mol%;

[0076] The spinel glass ceramic contains 15.00 wt % to 45.00 wt % of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramic;

[0077] Take W [(Zn,Mg)Al2O4] is the weight percentage of (Zn, Mg)Al2O4 phase in the spinel glass ceramic, W [Al2O3] is the weight percentage of Al2O3 in the spinel glass ceramic, W [MgO] is the weight percentage of MgO in the spinel glass ceramic, W [ZnO] is the weight percentage of ZnO in the spinel glass ceramic;

[0078] A=(1-W [(Zn,Mg)Al2O4] / 2)×W [Al2O3] / 2,

[0079] B=(1-W [(Zn,Mg)Al2O4] )×(W [MgO] +W [ZnO] ),

[0080] C=A / B, in the spinel glass-ceramics, 1.50≤C≤1.85.

[0081] It should be understood that the spinel glass ceramics of the present application are prepared by heat treatment of substrate glass, and therefore, based on the molar percentage of oxides, the composition of the spinel glass ceramics is the same as that of the substrate glass. That is, in the present application, the composition of the substrate glass for preparing the spinel glass ceramics, based on the molar percentage of oxides, includes: SiO2 35.00mol% to 60.00mol%, Al2O3 20.00mol% to 40.00mol%, ZrO2 2.00mol% to 8.00mol%, MgO 3.00mol% to 7.50mol%, ZnO 7.00mol% to 13.00mol%, Na2O 1.00mol% to 10.00mol%, Li2O 2.50mol% to 10.00mol%.

[0082] After heat treatment of the substrate glass that meets the above range is carried out to obtain a spinel glass ceramic that meets the specific crystal phase structure and has a specific glass network structure, the spinel glass ceramic can be chemically strengthened to obtain a strengthened spinel glass ceramic with an ultra-high compressive stress layer depth and a large deep stress.

[0083] In the glass system of the present application, SiO2 is a glass network forming oxide and an indispensable component of the glass network structure. An appropriate amount of SiO2 can increase the stability and mechanical strength of the glass, but an excessive amount of SiO2 will increase the viscosity of the substrate glass, making it more difficult to melt the glass, thereby reducing the formability of the substrate glass. Therefore, in the present application, in terms of mol% of the oxide, the content of SiO2 in the composition of the substrate glass or spinel glass ceramics is 35.00mol% to 60.00mol%.

[0084] In some embodiments of the present application, SiO2 content can be 35.00mol%, 37.00mol%, 40.00mol%, 42.00mol%, 45.00mol%, 47.00mol%, 50.00mol%, 52.00mol%, 55.00mol%, 57.00mol% or 60.00mol%, or the numerical value in the numerical range consisting of any two of the above numerical values ​​as endpoints. In some embodiments, SiO2 content can be 36.00mol%~58.00mol%, 38.00mol%~56.00mol%, 40.00mol%~52.00mol%, 42.00mol%~50.00mol% or 44.00mol%~48.00mol%.It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics of the desired performance of the application can be obtained.

[0085] In the glass system of the present application, an appropriate amount of Al2O3 can promote the precipitation of the main crystal phase, inhibit the precipitation of other impurity phases such as quartz, and is conducive to increasing the ion exchange rate during the chemical strengthening process. However, too much Al2O3 will cause the melting difficulty of the substrate glass to increase sharply, and it is easy to cause the substrate glass to have devitrification problems due to the excessively fast crystallization rate during the normal cooling process. Therefore, in the present application, in terms of mol% of the oxide, the content of Al2O3 in the composition of the substrate glass or spinel glass ceramics is 20.00mol% to 40.00mol%.

[0086] In some embodiments of the present application, the content of Al2O3 can be 20.00mol%, 21.00mol%, 22.00mol%, 23.00mol%, 24.00mol%, 25.00mol%, 26.00mol%, 27.00mol%, 28.00mol%, 29.00mol%, 30.00mol%, 31.00mol%, 32.00mol%, 33.00mol%, 34.00mol%, 35.00mol%, 36.00mol%, 37.00mol%, 38.00mol%, 39.00mol% or 40.00mol%, or a value within the numerical range consisting of any two of the above values ​​as endpoints. In some embodiments, the content of Al2O3 can be 22.00mol% to 38.00mol%, 24.00mol% to 36.00mol%, 26.00mol% to 34.00mol% or 28.00mol% to 32.00mol%. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the spinel glass ceramics with the desired properties of the present application can be obtained.

[0087] In the glass system of the present application, ZrO2 is an effective nucleating agent. During the heat treatment of the substrate glass, ZrO2 is first precipitated in the substrate glass in the form of crystals, and the ZrO2 crystals become crystal nuclei for the subsequent growth of the main crystal phase crystals. Within a certain glass composition range, the content of ZrO2 will affect the formation of the substrate glass, the crystal shape, crystal type and crystal size of the glass ceramics obtained by heat treatment of the substrate glass, etc. By regulating the composition of the substrate glass, the composition of the substrate glass meets the requirements of the appropriate amount of ZrO2, so that ZrO2 can be precipitated first, and then the main crystal phase spinel crystals grow. Too low a content of ZrO2 will affect the precipitation of the spinel crystal phase; while too high a content of ZrO2 will make it more difficult to melt the substrate glass, and it is easy to cause white unmelted materials to appear in the substrate glass. Therefore, in the present application, in terms of mol% of the oxide, the content of ZrO2 in the composition of the substrate glass or spinel glass ceramics is 2.00mol% to 8.00mol%.

[0088] In some embodiments of the present application, ZrO2 content can be 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol% or 8.00mol%, or the numerical value in the numerical range consisting of any two of the above numerical values ​​as endpoints. In some embodiments, ZrO2 content can be 2.50mol%~7.50mol%, 3.50mol%~7.00mol%, 4.50mol%~6.50mol% or 5.00mol%~6.00mol%.It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics of the desired performance of the application can be obtained.

[0089] In the glass system of the present application, MgO and ZnO are necessary components of the main crystalline phase spinel, which can promote the precipitation of spinel and reduce the difficulty of melting to a certain extent. However, excessive MgO and ZnO can easily lead to excessive growth of spinel grains, and it is difficult to obtain spinel glass ceramics with high transparency. Therefore, in the present application, in terms of mol% of oxide, in the composition of the substrate glass or spinel glass ceramics, the content of MgO is 3.00mol% to 7.50mol%, and the content of ZnO is 7.00mol% to 13.00mol%.

[0090] In some embodiments of the present application, the content of MgO can be 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol% or 7.50mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. In some embodiments, the content of MgO can be 3.50mol% to 7.50mol%, 4.50mol% to 7.00mol% or 5.00mol% to 6.00mol%. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0091] In some embodiments of the present application, the content of ZnO can be 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol%, 10.00mol%, 10.50mol%, 11.00mol%, 11.50mol%, 12.00mol%, 12.50mol% or 13.00mol%, or a numerical value in the numerical range consisting of any two of the above numerical values ​​as endpoints. In some embodiments, the content of ZnO can be 7.50mol% to 12.50mol%, 8.50mol% to 12.00mol%, 9.50mol% to 11.50mol% or 10.00mol% to 11.00mol%. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0092] In the glass system of the present application, the increase of Na2O content helps to obtain higher surface compressive stress, and at the same time helps to reduce the melting temperature of the substrate glass and the temperature of crystal precipitation when the substrate glass is used to prepare spinel glass ceramics. However, excessive Na2O is likely to cause the substrate glass to become ceramicized during annealing, or to cause the substrate glass to precipitate undesirable impurities during heat treatment to prepare spinel glass ceramics, thereby affecting the optical properties of spinel glass ceramics; while too low Na2O is likely to cause the heat treatment temperature of the substrate glass to increase when preparing spinel glass ceramics, or to cause direct phase separation or precipitation of undesirable impurities when preparing spinel glass ceramics from the substrate glass, thereby obtaining opaque glass ceramics. Therefore, in the present application, in terms of mol% of the oxide, the content of Na2O in the composition of the substrate glass or spinel glass ceramics is 1.00mol% to 10.00mol%.

[0093] In some embodiments of the present application, the content of Na2O can be 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol% or 10.00mol%, or a numerical value in the numerical range consisting of any two of the above numerical values ​​as endpoints. In some embodiments, the content of Na2O can be 1.50mol% to 9.50mol%, 2.50mol% to 9.00mol%, 3.50mol% to 8.50mol%, 4.50mol% to 7.50mol% or 5.00mol% to 7.00mol%. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired properties of the present application can be obtained.

[0094] In the glass system of the present application, the increase of Li2O content helps to obtain higher deep compressive stress, improve the Young's modulus of glass ceramics, and help to reduce the melting temperature of the substrate glass and the temperature of crystal precipitation when the substrate glass is used to prepare spinel glass ceramics. However, excessive Li2O can easily lead to ceramicization of the substrate glass during annealing, or can easily lead to the precipitation of undesirable impurities in the substrate glass during heat treatment to prepare spinel glass ceramics, or can easily lead to excessive crystal growth during heat treatment, thereby affecting the optical properties of spinel glass ceramics; while too low Li2O can easily lead to an increase in the heat treatment temperature when the substrate glass is used to prepare spinel glass ceramics, or can easily lead to a decrease in the deep stress that can be obtained during chemical strengthening of spinel glass ceramics. Therefore, in the present application, in terms of mol% of oxide, the content of Li2O in the composition of the substrate glass or spinel glass ceramics is 2.50mol% to 10.00mol%.

[0095] In some embodiments of the present application, the content of Li2O may be 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol% or 10.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. In some embodiments, the content of Li2O may be 3.00mol% to 9.50mol%, 3.50mol% to 9.00mol%, 4.00mol% to 8.50mol%, 4.50mol% to 7.50mol% or 5.00mol% to 7.00mol%. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired properties of the present application can be obtained.

[0096] In the present application, the spinel glass ceramics contain 15.00 wt% to 45.00 wt% of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramics. When the content of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramics is within the above range, it means that the spinel glass ceramics contain a large number of crystals with high hardness and high modulus, which can give the spinel glass ceramics high intrinsic strength or inherent strength. At the same time, by controlling the content of the (Zn, Mg)Al2O4 crystal phase, the spinel glass ceramics meet a specific crystal phase structure, which is beneficial to ensure that the spinel glass ceramics obtain an ideal stress structure after chemical strengthening.

[0097] In some embodiments of the present application, the crystal phase content of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramic is W [(Zn,Mg)Al2O4] % by weight, 33.00 wt. %, 35.00 wt. %, 38.00 wt. %, 40.00 wt. %, 43.00 wt. % or 45.00 wt. %, or a value within a range of values ​​consisting of any two of the above values ​​as endpoints. In some embodiments, the crystalline phase content W of the (Zn, Mg)Al2O4 crystalline phase in the spinel glass-ceramic is 15.00 wt. %, 18.00 wt. %, 20.00 wt. %, 23.00 wt. %, 25.00 wt. %, 28.00 wt. %, 30.00 wt. %, 33.00 wt. %, 35.00 wt. %, 38.00 wt. %, 40.00 wt. %, 43.00 wt. % or 45.00 wt. %, or a value within a range of values ​​consisting of any two of the above values ​​as endpoints. [(Zn,Mg)Al2O4] It may be 16.00 to 45.00 wt%, 18.00 to 43.00 wt%, 20.00 to 42.00 wt%, 22.00 to 40.00 wt%, or 25.00 to 35.00 wt%.

[0098] In some embodiments of the present application, take W [(Zn,Mg)Al2O4] is the weight percentage of (Zn, Mg)Al2O4 phase in spinel glass ceramics, W [Al2O3] is the weight percentage of Al2O3 in spinel glass ceramics, W [MgO] is the weight percentage of MgO in spinel glass ceramics, W [ZnO] is the weight percentage of ZnO in the spinel glass ceramic;

[0099] A=(1-W [(Zn,Mg)Al2O4] / 2)×W [Al2O3] / 2,

[0100] B=(1-W [(Zn,Mg)Al2O4] )×(W [MgO] +W [ZnO] ),

[0101] C=A / B, in spinel glass ceramics, 1.50≤C≤1.85.

[0102] By optimizing the composition and structure, the crystal phase content of the (Zn, Mg)Al2O4 crystal phase, and the contents of Al2O3, MgO, and ZnO in the spinel glass ceramics meet the range of the above-mentioned characteristic C, which can ensure that the spinel glass ceramics obtain the desired stress structure after chemical strengthening, thereby enabling the strengthened spinel glass ceramics to obtain high mechanical strength, especially excellent damage resistance. In some embodiments, in the above-mentioned spinel glass ceramics, calculated according to formula C, the value of C can be 1.52 to 1.82, 1.56 to 1.75, 1.60 to 1.70, or 1.62 to 1.68. In some embodiments, in the above-mentioned spinel glass ceramics, calculated according to formula C, the value of C can be 1.51, 1.53, 1.55, 1.58, 1.60, 1.62, 1.65, 1.68, 1.70, 1.72, 1.75, 1.78, 1.80, 1.82 or 1.85, or a value within the numerical range formed by any two of the above-mentioned values ​​as endpoints.

[0103] In some embodiments of the present application, W [Al2O3] It is 35.00wt%~50.00wt%.

[0104] In some embodiments of the present application, W [MgO] It is 2.50wt%~4.00wt%.

[0105] In some embodiments of the present application, W [ZnO] It is 9.50wt% to 14.50wt%.

[0106] In general, by making the composition and structure of spinel glass-ceramics satisfy the above-mentioned characteristics and making the crystal phase content of (Zn, Mg)Al2O4 crystal phase in spinel glass-ceramics satisfy the above-mentioned range, the spinel glass-ceramics can have a specific crystal phase structure and a specific glass network structure, thereby improving the chemical strengthening effect of spinel glass-ceramics, and enabling the spinel glass-ceramics to obtain a desired stress structure through chemical strengthening treatment, such as obtaining an ultra-high compressive stress layer depth and a larger deep stress, and obtaining a high stress level, thereby enabling the strengthened spinel glass-ceramics to obtain high mechanical strength and high damage resistance.

[0107] In some embodiments of the present application, in the spinel glass ceramics, the value of A is 10.00% to 25.00%, preferably 14.00% to 25.00%; and / or, the value of B is 7.50% to 12.50%, preferably 8.00% to 12.00%. By making the values ​​of A and B meet the above ranges, it is helpful to make the composition and structure of the spinel glass ceramics meet the value range of C, which helps to make the spinel glass ceramics meet a specific structure that is conducive to obtaining a desired stress level.

[0108] In some embodiments of the present application, the value of A can be 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00%, 16.00%, 17.00%, 18.00%, 19.00%, 20.00%, 21.00%, 22.00%, 23.00%, 24.00% or 25.00%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0109] In some embodiments of the present application, the value of B can be 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00% or 12.50%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0110] In some embodiments of the present application, the spinel glass ceramic further comprises a tetragonal ZrO2 crystal phase, and the total content of the (Zn, Mg)Al2O4 crystal phase and the tetragonal ZrO2 crystal phase accounts for 25.00 wt% to 70.00 wt% of the spinel glass ceramic, preferably 30.00 wt% to 50.00 wt% of the spinel glass ceramic. When the total crystal phase content W of the (Zn, Mg)Al2O4 crystal phase and the tetragonal ZrO2 crystal phase in the spinel glass ceramic is within the above range, it can ensure that the spinel glass ceramic has a large number of crystals that can hinder crack propagation, which is beneficial to improve the intrinsic strength or inherent strength of the spinel glass ceramic.

[0111] In some embodiments of the present application, the total crystalline phase content W of the (Zn, Mg)Al2O4 phase and the tetragonal ZrO2 phase can be 25.00 weight%, 28.00 weight%, 30.00 weight%, 33.00 weight%, 35.00 weight%, 38.00 weight%, 40.00 weight%, 43.00 weight%, 45.00 weight%, 48.00 weight%, 50.00 weight%, 53.00 weight%, 55.00 weight%, 58.00 weight%, 60.00 weight%, 63.00 weight%, 65.00 weight%, 68.00 weight% or 70.00 weight%, or a value within the numerical range formed by any two of the above values ​​as endpoints. In some embodiments, the total crystalline phase content W of the (Zn, Mg)Al2O4 crystalline phase and the tetragonal ZrO2 crystalline phase may be 26.00 wt% to 68.00 wt%, 28.00 wt% to 66.00 wt%, 30.00 wt% to 65.00 wt%, 32.00 wt% to 60.00 wt%, 35.00 wt% to 55.00 wt%, 38.00 wt% to 50.00 wt%, or 40.00 wt% to 48.00 wt%. It should be understood that in a specific embodiment, any of the above ranges may be combined with any other ranges as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0112] In some embodiments of the present application, in the spinel glass ceramics, the ratio of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase is 1.00 to 18.00, preferably 1.00 to 15.00. When the ratio of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase in the spinel glass ceramics (i.e., the mass ratio Z of the (Zn, Mg)Al2O4 crystal phase to the tetragonal ZrO2 crystal phase) is within the above range, the spinel glass ceramics can be endowed with a specific crystal phase structure, which is not only conducive to improving the intrinsic strength or inherent strength of the spinel glass ceramics, but also conducive to enabling the spinel glass ceramics to obtain a desired stress structure after chemical strengthening.

[0113] In some embodiments of the present application, the ratio (mass ratio Z) of (Zn, Mg)Al2O4 crystalline phase and tetragonal ZrO2 crystalline phase can be 1.00, 2.00, 3.00, 4.00, 5.00, 6.00, 7.00, 8.00, 9.00, 10.00, 11.00, 12.00, 13.00, 14.00, 15.00, 16.00, 17.00 or 18.00, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0114] In some embodiments of the present application, based on the quality of the spinel glass-ceramics, the crystalline phase content of the tetragonal ZrO2 crystalline phase is W [ZrO2] The tetragonal ZrO2 crystal phase and the (Zn, Mg)Al2O4 crystal phase jointly determine the crystal phase structure inside the spinel glass ceramics. By meeting a specific content range, it is beneficial to ensure the structural strength of the spinel glass ceramics and to ensure that the spinel glass ceramics obtain an ideal stress structure after chemical strengthening.

[0115] In some embodiments of the present application, the crystal phase content of the tetragonal ZrO2 crystal phase in the spinel glass ceramic is W [ZrO2] The amount may be 2.00%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00%, 10.00%, 11.00%, 12.00%, 13.00%, 14.00%, 15.00% or 16.00% by weight, or a value within a range of values ​​having any two of the above values ​​as endpoints.

[0116] In some embodiments of the present application, in the spinel glass ceramics, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is 3.0nm to 10.0nm, preferably 4.0nm to 8.0nm, more preferably 4.0nm to 7.5nm, and further preferably 4.5nm to 7.5nm. When the average crystal size of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramics is within the above range, it not only helps to improve the light transmittance of the spinel glass ceramics while ensuring the strength of the spinel glass ceramics, but also helps to improve the ion exchange performance of the spinel glass ceramics, so that it can obtain the desired stress level through chemical strengthening.

[0117] In some embodiments of the present application, the average crystal size of the (Zn, Mg)Al2O4 crystalline phase can be 3.0nm, 4.0nm, 4.2nm, 4.5nm, 4.8nm, 5.0nm, 5.2nm, 5.5nm, 5.8nm, 6.0nm, 6.2nm, 6.5nm, 6.8nm, 7.0nm, 7.2nm, 7.5nm, 8.0nm or 10.0nm, or a value within a numerical range consisting of any two of the above values ​​as endpoints. In some embodiments, the average crystal size of the (Zn, Mg)Al2O4 crystalline phase can be 4.0nm to 9.0nm, 4.5nm to 8.0nm, 4.5nm to 7.5nm or 4.5nm to 7.0nm. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0118] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics for preparing spinel glass-ceramics, measured in molar percentage of oxides, includes: SiO2 35.00mol%~60.00mol%, Al2O3 20.00mol%~40.00mol%, ZrO2 2.00mol%~8.00mol%, MgO 3.00mol%~7.50mol%, ZnO7.00mol%~13.00mol%, Na2O 1.00mol%~10.00mol%, Li2O 2.50mol%~10.00mol%, K2O0.00mol%~5.00mol%, CaO 0.00mol%~10.00mol%, B2O3 0.00mol%~10.00mol%, BaO0.00mol%~5.00mol%.

[0119] In addition to the ingredients necessary for preparing the spinel glass ceramics of the present application, in the glass system of the present application, K2O, CaO, B2O3 or BaO are optional components. The use of appropriate amounts can have a certain improvement effect on the forming effect, crystallization effect, chemical strengthening effect or optical effect of the spinel glass ceramics.

[0120] In the formulation system of the present application, K2O is an optional component that helps to improve the formability of the glass. + Radius larger than Na +, adding K2O in an appropriate amount can reduce the crystallization tendency of the base glass during the preparation process and increase the transparency and gloss of the spinel glass ceramic. In the present application, the content of K2O in the base glass or the spinel glass ceramic is 0.00mol% to 5.00mol%, calculated as mol% of the oxide. Adding K2O in this content range can achieve the above-mentioned effects without easily causing the chemical stability and hardness of the spinel glass ceramic to decrease, thereby avoiding the breakage of the spinel glass ceramic.

[0121] In some embodiments of the present application, the content of K2O can be 0.00mol%, 0.50mol%, 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol% or 5.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired properties of the present application can be obtained.

[0122] In the formulation system of the present application, B2O3 is an optional component that is beneficial to reducing the difficulty of melting the substrate glass. An appropriate amount of B2O3 is also beneficial to promoting the precipitation of spinel. However, too much B2O3 can easily lead to opacity or precipitation of impurities that affect the transparency of spinel glass ceramics when the substrate glass is heat-treated to prepare spinel glass ceramics. In the present application, the content of B2O3 can be 0.00mol% to 10.00mol%, calculated as mol% of the oxide.

[0123] In some embodiments of the present application, the content of B2O3 can be 0.00mol%, 0.50mol%, 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol% or 10.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0124] In the formulation system of the present application, BaO is an optional component that is beneficial to improving the melting effect of the substrate glass. An appropriate amount of BaO can also inhibit the growth of grains to a certain extent, thereby improving the optical properties of the spinel glass ceramics to a certain extent. However, too much BaO is likely to affect the chemical strengthening effect of the spinel glass ceramics, greatly reducing the stress level that can be obtained. In the present application, the content of BaO is 0.00mol% to 5.00mol% in terms of mol% of the oxide.

[0125] In some embodiments of the present application, the content of BaO can be 0.00mol%, 0.50mol%, 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol% or 5.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0126] In the formulation system of the present application, CaO is an optional component that is beneficial to reducing the viscosity of the glass liquid and enhancing the formability of the substrate glass. An appropriate amount of CaO is also beneficial to increasing the strain point and Young's modulus, and is beneficial to improving the ion exchange capacity of the spinel glass ceramic. At the same time, an appropriate amount of CaO can also increase the gloss and transparency of the substrate glass, reduce the crystallization tendency of the substrate glass, and slow down the hardening speed of the substrate glass. However, too much CaO can easily lead to an increase in the glass density, thereby affecting the ion exchange performance of the spinel glass ceramic. In the present application, the content of CaO is 0.00mol% to 10.00mol% in terms of mol% of the oxide.

[0127] In some embodiments of the present application, the content of CaO can be 0.00mol%, 0.50mol%, 1.00mol%, 1.50mol%, 2.00mol%, 2.50mol%, 3.00mol%, 3.50mol%, 4.00mol%, 4.50mol%, 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol% or 10.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0128] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics for preparing spinel glass-ceramics, measured in molar percentage of oxides, includes: SiO2 35.00mol%~60.00mol%, Al2O3 20.00mol%~40.00mol%, ZrO2 2.00mol%~8.00mol%, MgO 4.00mol%~7.00mol%, ZnO9.00mol%~12.00mol%, Na2O 2.00mol%~10.00mol%, Li2O 3.00mol%~10.00mol%, K2O0.00mol%~5.00mol%, CaO 0.00mol%~10.00mol%, B2O3 0.00mol%~10.00mol%, BaO0.00mol%~5.00mol%. By properly adjusting the content of MgO, ZnO, Li2O or Na2O, it helps to ensure that the main crystalline phase content in the spinel glass-ceramics meets the desired level, and also helps to ensure that the spinel glass-ceramics achieves the desired chemical strengthening effect, thereby obtaining strengthened spinel glass-ceramics with a high stress level.

[0129] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics for preparing spinel glass-ceramics, measured in molar percentage of oxides, includes: SiO2 35.00mol%~50.00mol%, Al2O3 25.00mol%~35.00mol%, ZrO2 3.00mol%~5.00mol%, MgO 4.00mol%~7.00mol%, ZnO9.00mol%~12.00mol%, Na2O 2.00mol%~10.00mol%, Li2O 3.00mol%~10.00mol%, K2O0.00mol%~5.00mol%, CaO 0.00mol%~10.00mol%, B2O3 0.00mol%~10.00mol%, BaO0.00mol%~5.00mol%. By properly adjusting the content of each necessary oxide, it helps to ensure that the spinel glass-ceramics achieves the desired crystal phase structure and glass network structure that can achieve high stress levels, which is conducive to obtaining strengthened spinel glass-ceramics with high stress levels.

[0130] In some embodiments of the present application, the composition of the substrate glass or spinel glass ceramic, measured in terms of the molar percentage of each oxide in the composition, satisfies: 1.30≤ZnO / MgO≤2.50; by ensuring that ZnO and MgO satisfy a specific content relationship, it is helpful to ensure the formation of the desired main crystalline phase structure.

[0131] In some embodiments of the present application, the value of ZnO / MgO can be 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.00, 2.10, 2.20, 2.30, 2.40 or 2.50, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0132] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics, measured in terms of the molar percentage of each oxide in the composition, satisfies the following conditions: 0.05≤Li2O / (Al2O3-(MgO+ZnO)+SiO2)≤0.20; by making Li2O, Al2O3, MgO, ZnO and SiO2 satisfy a specific content relationship, it helps to improve the ion exchange properties of the spinel glass-ceramics, and helps to enable the spinel glass-ceramics to obtain a high compressive stress layer depth and a larger deep stress through chemical strengthening, thereby helping to improve the mechanical strength and damage resistance of the spinel glass-ceramics, especially to improve its drop impact resistance.

[0133] In some embodiments of the present application, the value of Li2O / (Al2O3-(MgO+ZnO)+SiO2) can be 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19 or 0.20, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass-ceramics with the required properties of the present application can be obtained.

[0134] In some embodiments of the present application, the composition of the substrate glass or spinel glass ceramics, measured in terms of the molar percentage of each oxide in the composition, satisfies the following condition: 0.19≤(Al2O3-(MgO+ZnO)) / SiO2≤0.60; by ensuring that Al2O3, MgO, ZnO and SiO2 satisfy a specific content relationship, it is possible to ensure that there is an appropriate amount of Al in the residual glass phase of the spinel glass ceramics. On the one hand, this helps to exert the synergistic effect of Si and Al, allowing the residual glass phase to form a specific network structure, thereby improving the intrinsic strength of the spinel glass ceramics; on the other hand, it helps to promote ion exchange and improve the chemical strengthening effect of the spinel glass ceramics.

[0135] In some embodiments of the present application, the value of (Al2O3-(MgO+ZnO)) / SiO2 can be 0.19, 0.20, 0.23, 0.25, 0.28, 0.30, 0.33, 0.35, 0.38, 0.40, 0.43, 0.45, 0.48, 0.50, 0.53, 0.55, 0.58 or 0.60, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges as long as the spinel glass ceramics with the required properties of the present application can be obtained.

[0136] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics, measured in terms of the molar percentage of each oxide in the composition, satisfies the following conditions: 0.26≤Na2O / Li2O≤3.00; by ensuring that Na and Li satisfy a specific content relationship, it helps to ensure that the spinel glass-ceramics obtain the desired surface stress level and deep stress level after chemical strengthening, thereby obtaining the desired stress structure and achieving high mechanical strength and high damage resistance.

[0137] In some embodiments of the present application, the value of Na2O / Li2O can be 0.26, 0.30, 0.50, 0.80, 1.00, 1.20, 1.50, 1.80, 2.00, 2.20, 2.30, 2.50, 2.80 or 3.00, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0138] By making the composition of the spinel glass ceramics of the present application satisfy at least one of the above-mentioned relationships ZnO / MgO, Li2O / (Al2O3-(MgO+ZnO)+SiO2), (Al2O3-(MgO+ZnO)) / SiO2, and Na2O / Li2O, it helps to further adjust the network structure and crystal phase structure of the spinel glass ceramics, so that the spinel glass ceramics form a specific microstructure that helps to obtain the desired stress level.

[0139] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics, measured in terms of the molar percentage of each oxide in the composition, also satisfies the following conditions: 12.00mol%≤ZnO+MgO≤20.00mol%, preferably, 13.00mol%≤ZnO+MgO≤17.30mol%; by having a sufficient amount of ZnO and MgO in the composition, it helps to ensure that a sufficient amount of main crystalline phase can be precipitated in the spinel glass-ceramics, thereby forming a desired crystalline phase structure.

[0140] In some embodiments of the present application, the value of ZnO+MgO can be 12.00mol%, 13.00mol%, 13.30mol%, 13.50mol%, 13.80mol%, 14.00mol%, 14.30mol%, 14.50mol%, 14.80mol%, 15.00mol%, 15.30mol%, 15.50mol%, 15.80mol%, 16.00mol%, 16.30mol%, 16.50mol%, 16.80mol%, 17.00mol%, 17.30mol%, 18.00mol%, 19.00mol% or 20.00mol%, or a numerical value within a numerical range consisting of any two of the above numerical values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0141] In some embodiments of the present application, the composition of the substrate glass or spinel glass-ceramics, measured in terms of the molar percentage of each oxide in the composition, also satisfies the following conditions: 9.00mol%≤Al2O3-(MgO+ZnO)≤22.00mol%, preferably, 10.00mol%≤Al2O3-(MgO+ZnO)≤20.00mol%; by making the content of Al2O3 in the composition higher than the sum of the contents of MgO and ZnO, while ensuring the formation of the main crystalline phase, an appropriate amount of Al can be present in the residual glass phase, which, on the one hand, helps to exert the synergistic effect of Si and Al and form a specific network structure of the residual glass phase, thereby improving the intrinsic strength of the spinel glass-ceramics; on the other hand, it helps to promote ion exchange and improve the chemical strengthening effect of the spinel glass-ceramics.

[0142] In some embodiments of the present application, the value of Al2O3-(MgO+ZnO) can be 9.00mol%, 10.00mol%, 11.00mol%, 12.00mol%, 13.00mol%, 14.00mol%, 15.00mol%, 16.00mol%, 17.00mol%, 18.00mol%, 19.00mol%, 20.00mol%, 21.00mol% or 22.00mol%, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0143] In some embodiments of the present application, the composition of the substrate glass or spinel glass ceramics, measured by the molar percentage of each oxide in the composition, also satisfies: 5.00mol%≤Na2O+Li2O≤15.00mol%, preferably, 6.00mol%≤Na2O+Li2O≤13.50mol%. By having sufficient amounts of Na and Li in the composition, it is helpful to improve the ion exchange properties of the spinel glass ceramics, thereby ensuring that the spinel glass ceramics can obtain the desired surface stress level and deep stress level after chemical strengthening, thereby obtaining the desired stress structure, and achieving high mechanical strength and high damage resistance of the strengthened spinel glass ceramics.

[0144] In some embodiments of the present application, the value of Na2O+Li2O can be 5.00mol%, 5.50mol%, 6.00mol%, 6.50mol%, 7.00mol%, 7.50mol%, 8.00mol%, 8.50mol%, 9.00mol%, 9.50mol%, 10.00mol%, 10.50mol%, 11.00mol%, 11.50mol%, 12.00mol%, 12.50mol%, 13.00mol%, 13.50mol%, 14.00mol%, 14.50mol% or 15.00mol%, or a numerical value within a numerical range consisting of any two of the above numerical values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0145] By making the spinel glass ceramics of the present application satisfy at least one of the above-mentioned relationships ZnO+MgO, Al2O3-(MgO+ZnO), and Na2O+Li2O, it helps to obtain a high content of (Zn, Mg)Al2O4 crystal phase with high hardness and high modulus to further improve the intrinsic strength or inherent strength of the spinel glass ceramics, or, it helps to further improve the ion exchange effect of the spinel glass ceramics to obtain the desired stress level.

[0146] In the present application, each substance in the above-mentioned relationship formulas ZnO / MgO, Li2O / (Al2O3-(MgO+ZnO)+SiO2), (Al2O3-(MgO+ZnO)) / SiO2, Na2O / Li2O, ZnO+MgO, Al2O3-(MgO+ZnO), and Na2O+Li2O represents the molar percentage content of the corresponding substance. For example, ZnO represents the molar percentage content of ZnO, MgO represents the molar percentage content of MgO, and so on. This application will not go into details one by one.

[0147] In some embodiments of the present application, the spinel glass ceramic is transparent in the visible light range. In the present application, the visible light range refers to light in the wavelength range of 360nm to 740nm; "transparent in the visible light range" means that the average transmittance to visible light is greater than 80%.

[0148] In some embodiments of the present application, the transmittance of 0.7 mm thick spinel glass ceramics under 550 nm wavelength light is greater than or equal to 85%. The transmittance of 0.7 mm thick spinel glass ceramics under 550 nm wavelength light is within the above range, indicating that the spinel glass ceramics of the present application have high light transmittance. At the same time, the spinel glass ceramics of the present application can also obtain high mechanical strength and high damage resistance through chemical strengthening treatment, and have excellent drop impact resistance, which effectively broadens the application scenarios and application fields of the spinel glass ceramics of the present application. In some embodiments of the present application, the transmittance T can be 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98% or 99%, or a value within the numerical range consisting of any two of the above values ​​as endpoints.

[0149] By making the spinel glass ceramics meet a specific crystal phase structure, on the one hand, it is beneficial for the spinel glass ceramics to obtain high intrinsic strength, and on the other hand, it is beneficial to improve the chemical strengthening effect of the spinel glass ceramics, so that it can obtain ultra-high compressive stress layer depth and large deep stress through chemical strengthening, which is beneficial to improve the mechanical strength and damage resistance of the spinel glass ceramics. The relevant characteristics of the X-ray diffraction spectrum can reflect the crystal phase structure of the glass ceramics, including crystal phase composition, crystal size, etc.

[0150] In some embodiments of the present application, in the X-ray diffraction spectrum of the spinel glass ceramic, the peak with the peak intensity maximum in the characteristic peak with a 2θ angle in the range of 28° to 32° is taken as the first characteristic peak, and the peak with the peak intensity maximum in the characteristic peak with a 2θ angle in the range of 36° to 38° is taken as the second characteristic peak, and the peak intensity ratio X of the first characteristic peak and the second characteristic peak is 0.80 to 1.50, and the peak intensity ratio X is preferably 0.85 to 1.30. The peak intensity ratio X of the spinel glass ceramic is within the above range, indicating that the spinel glass ceramic has obtained a suitable crystal integrity, which helps to ensure that the spinel glass ceramic obtains a better optical effect and strengthening effect. In some embodiments of the present application, the peak intensity ratio X can be 0.80, 0.90, 1.00, 1.10, 1.20, 1.30, 1.40 or 1.50, or a value within the numerical range formed by any two of the above values ​​as endpoints. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired properties of the present application can be obtained.

[0151] In some embodiments of the present application, in the X-ray diffraction pattern of the spinel glass ceramic, the

[400] crystal plane characteristic peak of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 44° to 46°, the

[311] crystal plane characteristic peak of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 34° to 38°, and the

[440] crystal plane characteristic peak of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle of 64° to 67°; the half-peak width W of the

[400] crystal plane characteristic peak is

[400] 0.650° to 1.800°, preferably W

[400] 0.900° to 1.600°; the half-peak width W of the characteristic peak of the

[311] crystal plane

[311] 0.900° to 2.800°, preferably W

[311] 1.100° to 2.230°; the half-peak width W of the characteristic peak of the

[440] crystal plane

[440] 0.750° to 2.000°, preferably W

[440] The W of spinel glass ceramics is 0.900° to 1.600°.

[400] , W

[311] , W

[440] Within the above range, it is shown that the (Zn, Mg)Al2O4 crystal phase in the crystal phase structure of the spinel glass ceramic has a suitable average crystal size and satisfies a specific crystal phase structure, which is not only conducive to giving the spinel glass ceramic a high intrinsic strength or inherent strength, but also conducive to ensuring that the spinel glass ceramic obtains an ideal stress structure after chemical strengthening. At the same time, it is helpful for the spinel glass ceramic to obtain the desired optical properties.

[0152] In some embodiments of the present application, W

[400] The value of can be 0.650°, 0.700°, 0.800°, 0.900°, 1.000°, 1.100°, 1.200°, 1.300°, 1.400°, 1.500°, 1.600°, 1.700° or 1.800°, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0153] In some embodiments of the present application, W

[311] The value of can be 0.900°, 1.000°, 1.100°, 1.200°, 1.300°, 1.400°, 1.500°, 1.600°, 1.700°, 1.800°, 1.900°, 2.000°, 2.100°, 2.200°, 2.2300°, 2.300°, 2.400°, 2.500°, 2.600°, 2.700°, or 2.800°, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0154] In some embodiments of the present application, W

[440] The value of can be 0.750°, 0.800°, 0.900°, 1.000°, 1.100°, 1.200°, 1.300°, 1.400°, 1.500°, 1.600°, 1.700°, 1.800°, 1.900° or 2.000°, or a value within a numerical range consisting of any two of the above values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the spinel glass ceramics with the desired performance of the present application can be obtained.

[0155] The present application has no particular restriction on the thickness t of the spinel glass ceramics, as long as the purpose of the present application can be achieved. For example, the thickness t of the spinel glass ceramics satisfies: 0.2 mm ≤ t ≤ 5.0 mm, preferably 0.2 mm ≤ t ≤ 2.0 mm.

[0156] In the present application, the spinel glass ceramics or the strengthened spinel glass ceramics prepared therefrom may be 2D, 2.5D, 3D or special-shaped glass products. In the present application, the spinel glass ceramics or the strengthened spinel glass ceramics prepared therefrom may be glass products of equal thickness or unequal thickness.

[0157] In some embodiments of the present application, the spinel glass ceramics in any of the aforementioned embodiments can be subjected to chemical strengthening treatment to produce reinforced spinel glass ceramics having high mechanical strength and high damage resistance, wherein the reinforced spinel glass ceramics comprises a compressive stress layer region extending from the surface of the reinforced spinel glass ceramics to the compression depth and has a tensile stress layer region inside.

[0158] It should be understood that after the chemical strengthening treatment and the ion exchange process, the composition of the glass ceramic product at the surface may be different from the composition of the glass ceramic before the ion exchange process. This is because, when the ion exchange is performed, a type of alkali metal ion (e.g., Li+) at the surface of the newly formed glass ceramic (e.g., the spinel glass ceramic in the present application) is + Or Na + ) are replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced. However, in the embodiment, the glass composition and phase assembly at the center of the depth of the glass ceramic product or near the center of the depth will still be the composition of the newly formed glass ceramic. That is to say, in the present application, the composition and phase assembly at the center of the strengthened spinel glass ceramic obtained by chemical strengthening are the same as the spinel glass ceramic in the present application.

[0159] At the same time, in the spinel glass ceramics of the present application, the main crystal phase (Zn, Mg) Al2O4 crystal phase and the secondary crystal phase tetragonal ZrO2 crystal phase do not contain alkali metal ions, so they do not participate in the ion exchange during the chemical strengthening process. Based on this, the crystal phase structure of the strengthened spinel glass ceramics obtained by chemical strengthening in the present application is basically the same as that of the spinel glass ceramics. That is, the crystal phase content, crystal composition, crystal size, and X-ray diffraction spectrum characteristics of the strengthened spinel glass ceramics obtained by the chemical strengthening process of the present application are basically the same as those of the spinel glass ceramics of the present application, such as Fig. 9 As shown in FIG. 1 , in Example 1, the XRD patterns of the spinel glass ceramics before chemical strengthening and the strengthened spinel glass ceramics after chemical strengthening are substantially the same. Fig.10 As shown, in the present application, the transmittance of the spinel glass ceramics before and after chemical strengthening is basically the same as the transmittance of the strengthened spinel glass ceramics. That is to say, in the present application, by using spinel glass ceramics with high transmittance, chemical strengthening treatment can be performed to obtain strengthened spinel glass ceramic products with the same excellent transmittance.

[0160] In some embodiments of the present application, the depth of the compressive stress layer DOL_0 of the above-mentioned strengthened spinel glass-ceramics is ≥0.21t, preferably, 0.21t≤DOL_0≤0.25t, and t is the thickness of the strengthened spinel glass-ceramics. Exemplarily, when the thickness t of the strengthened glass-ceramics is 0.7mm, 147μm≤DOL_0≤175μm, specifically, DOL_0 can be 147μm, 154μm, 161μm, 168μm or 175μm, or a value within the numerical range formed by any two of the above values ​​as endpoints. The strengthened spinel glass-ceramics has the above-mentioned DOL_0, which means that the strengthened spinel glass-ceramics has an ultra-high depth of compressive stress layer, which can more advantageously offset the energy that drives crack propagation during the external impact process.

[0161] In some embodiments of the present application, the CS_50 of the above-mentioned strengthened spinel glass-ceramics is ≥100MPa, preferably, 100MPa≤CS_50≤250MPa. The range of CS_50 of the strengthened spinel glass-ceramics is within the above range, indicating that the strengthened spinel glass-ceramics has a high compressive stress at a depth of 50μm from the surface, which further indicates that the strengthened spinel glass-ceramics has a high surface stress level, thereby effectively improving the drop impact resistance of the strengthened spinel glass-ceramics.

[0162] In some embodiments of the present application, the |CT_AV| of the strengthened spinel glass-ceramics is ≥ 70 MPa, preferably, 70 MPa≤|CT_AV|≤110 MPa. The strengthened spinel glass-ceramics having the above |CT_AV| indicates that the spinel glass-ceramics has a large deep stress, which directly reflects that the strengthened spinel glass-ceramics has a high surface stress level, which is conducive to offsetting more external impact energy.

[0163] In some embodiments of the present application, the |CT_CV| of the above-mentioned strengthened spinel glass-ceramics is ≥80MPa, preferably, 80MPa≤|CT_CV|≤150MPa. The |CT_CV| of the strengthened spinel glass-ceramics is within the above range, which indicates that the strengthened spinel glass-ceramics has a large deep stress, and also reflects that the strengthened spinel glass-ceramics has a high surface stress level, which is conducive to offsetting more external impact energy.

[0164] In some embodiments of the present application, the Vickers hardness of the strengthened spinel glass-ceramic is greater than or equal to 790 kgf / mm 2 , preferably 790kgf / mm 2 Up to 1000kgf / mm 2 The Vickers hardness of the strengthened spinel glass-ceramics is within the above range, indicating that the strengthened spinel glass-ceramics has high hardness, thereby ensuring that it has excellent mechanical properties.

[0165] In some embodiments of the present application, the fracture toughness of the reinforced spinel glass-ceramic is greater than or equal to 1.00 MPa·m 1 / 2 , preferably greater than or equal to 1.20 MPa·m 1 / 2 In some embodiments, the fracture toughness of the reinforced spinel glass-ceramic may be 1.00 to 2.00 MPa·m 1 / 2 , 1.20MPa·m 1 / 2 ~2.00MPa·m 1 / 2 or 1.55MPa·m 1 / 2 ~2.00MPa·m 1 / 2 The fracture toughness of the strengthened spinel glass-ceramics is within the above range, indicating that the strengthened spinel glass-ceramics has high fracture toughness, thereby ensuring that it has excellent mechanical properties.

[0166] In some embodiments of the present application, the above-mentioned reinforced spinel glass-ceramics with a thickness of 0.7 mm are subjected to a drop resistance test using 80-mesh sandpaper, and the average sandpaper drop resistance height of the reinforced spinel glass-ceramics is greater than or equal to 1.00 m, and preferably the average sandpaper drop resistance height is greater than or equal to 1.40 m. In some embodiments, the above-mentioned reinforced spinel glass-ceramics with a thickness of 0.7 mm are subjected to a drop resistance test using 80-mesh sandpaper, and the average sandpaper drop resistance height of the reinforced spinel glass-ceramics can be 1.00 m to 2.50 m, 1.40 m to 2.50 m, or 1.50 mm to 2.50 m. The average sandpaper drop resistance height H of the 0.7 mm thick reinforced spinel glass-ceramics is within the above range, indicating that the reinforced spinel glass-ceramics has high damage resistance, especially excellent drop impact resistance.

[0167] In some embodiments of the present application, a 10 mm diameter round head metal pressure rod is used to extrude the 0.7 mm thick reinforced spinel glass ceramics, and the single rod static pressure strength that the reinforced spinel glass ceramics can withstand is tested. The single rod static pressure strength that the reinforced spinel glass ceramics can withstand is greater than 500 N, preferably greater than 550 N. This shows that the reinforced spinel glass ceramics have good anti-extrusion performance and good compressive resistance.

[0168] The preparation method of the spinel glass ceramic in any of the aforementioned embodiments of the present application may include but is not limited to the following steps:

[0169] (1) Preparation of substrate glass: Expressed as the molar percentage of oxides, the substrate glass or spinel glass-ceramic is prepared according to the composition of any of the aforementioned embodiments. After uniform mixing, the substrate glass is prepared by conventional methods known in the art. The substrate glass preparation methods include but are not limited to float, overflow, rolling, casting, continuous melting and the like. The present application does not limit the parameters in the preparation process, as long as the substrate glass having the required performance of the present application can be obtained.

[0170] (2) Preparation of spinel glass ceramics: heat-treating the substrate glass obtained in step (1), wherein the heat treatment includes but is not limited to one-step heat treatment or multiple-step heat treatment, to obtain the spinel glass ceramics in any of the aforementioned embodiments of the present application. The present application does not limit the parameters in the preparation process, as long as the spinel glass ceramics with the required performance of the present application can be obtained.

[0171] In some embodiments of the present application, the preparation method of the substrate glass in the above step (1) may include but is not limited to the following steps: prepare the ingredients according to the composition of the substrate glass or spinel glass ceramic in any of the above embodiments, mix them evenly, melt, form, cool, and anneal to obtain the substrate glass. The present application has no special restrictions on the melting temperature and time, as long as each component can be fully melted. Preferably, the melting temperature is 1550℃~1800℃, and the preferred melting time is 3h~12h. The present application does not limit the molding method, as long as the purpose of the present application can be achieved, for example, it can be cast into a molding mold to form a glass brick. The present application does not limit the cooling temperature, as long as the purpose of the present application can be achieved. Preferably, the cooling temperature is 800℃~1000℃. The present application does not limit the annealing temperature and time, as long as the purpose of the present application can be achieved. Preferably, the annealing temperature is 500℃~700℃ and the time is 20h~26h.

[0172] In some embodiments of the present application, the heat treatment in the above step (2) includes a nucleation treatment and a crystallization treatment. Preferably, the temperature T1 of the nucleation treatment is 600°C to 850°C, and more preferably T1 is 650°C to 850°C. In some embodiments, the temperature T1 of the nucleation treatment can be 600°C, 625°C, 650°C, 675°C, 680°C, 690°C, 700°C, 710°C, 720°C, 725°C, 730°C, 740°C, 750°C, 775°C, 800°C, 825°C or 850°C, or a value within the numerical range consisting of any two of the above values ​​as endpoints. Preferably, the nucleation treatment time t1 is 0h to 72h, more preferably t1 is 0h to 24h, and more preferably t1 is 0h to 8h. In some embodiments, the nucleation treatment time t1 can be 0h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 16h, 24h, 32h, 40h, 48h, 56h, 64h or 72h, or a value within a numerical range consisting of any two of the above values ​​as endpoints. Preferably, the temperature T2 of the crystallization treatment is 700°C to 1000°C. In some embodiments, the temperature T2 of the crystallization treatment can be 700°C, 710°C, 720°C, 730°C, 740°C, 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C, 850°C, 875°C, 900°C, 925°C, 950°C, 975°C or 1000°C, or a value within a numerical range consisting of any two of the above values ​​as endpoints. Preferably, the crystallization treatment time t2 is 10 min to 400 min, preferably t2 is 10 min to 120 min. In some embodiments, the crystallization treatment time t2 can be 10 min, 20 min, 30 min, 40 min, 50 min, 60 min, 70 min, 80 min, 90 min, 100 min, 110 min, 120 min, 150 min, 170 min, 200 min, 220 min, 250 min, 280 min, 300 min, 320 min, 350 min, 370 min or 400 min, or a value within the numerical range consisting of any two of the above values ​​as endpoints.

[0173] In the present application, when the substrate glass is heat-treated to prepare spinel glass ceramics, a one-step heat treatment can be performed, or a two-step or multi-step heat treatment can be performed. If a one-step heat treatment is performed, it means that the nucleation treatment is not performed separately, and a one-step heating is performed directly, and the nucleation and target crystal growth are performed at the temperature reached by the one-step heating process, which can be understood as directly performing a crystallization treatment. If a two-step heat treatment is performed, it means that a two-step heating process is performed, first a nucleation treatment, i.e., a nucleation treatment, is performed, and then a target crystal growth treatment, i.e., a crystallization treatment, is performed. If a multi-step heat treatment is performed, then the nucleation treatment stage and / or the crystallization treatment stage adopts a step-by-step heating method, that is, the entire heat treatment process will be heated multiple times (more than twice).

[0174] In the present application, the nucleation treatment is to increase the temperature to a specified nucleation treatment temperature (also called nucleation temperature), and after reaching the nucleation treatment temperature, keep it warm for a certain time, and the holding time here is the nucleation treatment time (also called nucleation time); the crystallization treatment is to increase the temperature to a specified crystallization treatment temperature (also called crystallization temperature), and after reaching the crystallization treatment temperature, keep it warm for a certain time, and the holding time here is the crystallization treatment time (also called crystallization time).

[0175] In some embodiments of the present application, in step (2), when heat treatment is performed, the heating rate is preferably controlled to be 5K / min to 15K / min, preferably 5K / min to 10K / min. In some embodiments, the heating rate may be 5K / min, 6K / min, 7K / min, 8K / min, 9K / min, 10K / min, 11K / min, 12K / min, 13K / min, 14K / min or 15K / min, or a value within a numerical range consisting of any two of the above values ​​as endpoints.

[0176] In some embodiments of the present application, the spinel glass ceramics obtained in the above step (2) are subjected to chemical strengthening treatment to obtain the strengthened spinel glass ceramics in any of the above embodiments.

[0177] In some embodiments of the present application, the salt bath for chemical strengthening treatment of spinel glass ceramics is a molten salt containing potassium salt and / or sodium salt, and the potassium salt includes one or more of potassium nitrate, potassium sulfate, and potassium carbonate, preferably potassium nitrate; the sodium salt includes at least one of sodium nitrate, sodium sulfate, and sodium carbonate, preferably sodium nitrate. Preferably, the temperature T3 of the salt bath for chemical strengthening treatment is 380℃~600℃, preferably T3 is 400℃~550℃, and more preferably T3 is 400℃~500℃. In some embodiments, the temperature T3 of the salt bath for chemical strengthening treatment can be 380℃, 400℃, 425℃, 450℃, 475℃, 500℃, 525℃, 550℃, 575℃ or 600℃, or a value within the numerical range consisting of any two of the above values ​​as endpoints. Preferably, the time t3 of chemical strengthening treatment is 1h~48h, preferably t3 is 2h~24h, and more preferably t3 is 2h~15h. In some embodiments, the time t3 of the chemical strengthening treatment can be 1h, 4h, 8h, 12h, 16h, 20h, 24h, 28h, 32h, 36h, 40h, 44h or 48h, or a value within a numerical range consisting of any two of the above values ​​as endpoints. In some embodiments of the present application, a certain amount (e.g., 0wt% to 0.5wt%) of lithium salt can be added to the salt bath. By adopting the above-mentioned chemical strengthening treatment process scheme to strengthen spinel glass-ceramics with specific composition and structure, it is possible to obtain strengthened spinel glass-ceramics with excellent surface stress characteristics and excellent deep stress characteristics, thereby ensuring that the obtained strengthened spinel glass-ceramics have high mechanical strength and excellent damage resistance.

[0178] It should be understood that when the chemical strengthening treatment is performed, one step of chemical strengthening treatment may be performed, or two or more steps of chemical strengthening treatment may be performed. In the present application, the temperature of the chemical strengthening treatment is the temperature of the salt bath; when the chemical strengthening treatment includes two or more steps, the time of the chemical strengthening treatment is the sum of the time of each step of the chemical strengthening treatment. In some embodiments of the present application, when the chemical strengthening treatment includes two or more steps, the temperature and time of the chemical strengthening treatment of each step may be the same or different.

[0179] In the present application, the spinel glass ceramics in any of the aforementioned embodiments can be used to produce glass devices with high strength. For example, the glass devices may include but are not limited to worktops, other surfaces, appliance doors, floor tiles, wall panels, storage containers, mobile phone screens, mobile phone back panels, electronic device frames, vehicle windshields, aircraft windshields or aircraft windshields, etc. The spinel glass ceramics provided in the present application can obtain a high stress level after chemical strengthening treatment, thereby obtaining high mechanical strength and high damage resistance, especially excellent drop impact resistance. Glass devices prepared by chemically strengthening the spinel glass ceramics of the present application can ensure excellent mechanical properties.

[0180] In the present application, the spinel glass ceramic in any of the aforementioned embodiments can be used in electronic devices.

[0181] In some embodiments of the present application, the electronic device includes at least one of a mobile phone, a tablet computer, a smart wear, a display and a TV. For example, the electronic device may include but is not limited to a mobile phone, a tablet computer, a smart wear, a display or a TV, etc. Smart wear may include but is not limited to an electronic watch, a smart bracelet, a smart watch, smart glasses, etc., and the display may include but is not limited to a high-definition display, a car display, an aircraft display, etc. Exemplarily, the electronic device may include a housing and an electronic component partially located in the housing, the housing includes a front surface, a rear surface and a side surface, the electronic component includes a display device, the display device is located at the front surface of the housing or adjacent to the front surface, and the spinel glass ceramic provided in the present application can be applied to the front surface and / or rear surface and / or side surface of the housing after chemical strengthening. In some embodiments, the front surface and / or rear surface of the housing may be of equal thickness or unequal thickness. In some embodiments, the front surface and / or rear surface of the housing may be 2D, 2.5D, 3D or shaped.

[0182] Test method:

[0183] 1. X-ray diffraction (XRD) test

[0184] The sample to be tested was crushed and ground into a sample with a particle size of less than 75 μm. The ground sample was tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The XRD diffraction data was then analyzed using JADE Standard 8.6 software to obtain the crystalline phase of the sample. The X-ray diffractometer was Shimadzu XRD-6100, the incident angle range used in the test was 2θ=10°~80°, the scanning speed was 6° / min, the operating voltage was 40 kV, and the operating current was 30 mA. Among them, the sample to be tested was a chemically strengthened glass ceramic or a strengthened glass ceramic.

[0185] Average crystal size: The average crystal size of the sample can be calculated using the result data obtained from the XRD test according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the X-ray wavelength, λ = 0.154056nm, β is the half-peak width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW file (diffraction spectrum) output by the XRD instrument is curve-fitted in the JADEStandard 8.6 software, and Jade outputs the fitting report. According to the angle 2θ value and Peak FWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted into radians: β = (FWHM / 180×3.14), and the crystal size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size.

[0186] Average crystal size of (Zn, Mg)Al2O4 crystal phase: The RAW file (diffraction pattern) output by the XRD instrument was used for phase retrieval and curve fitting in JADE Standard 8.6 software. In the output fitting report, the angle 2θ values ​​and Peak FWHM values ​​corresponding to the three diffraction peaks of (Zn, Mg)Al2O4 crystal phase in the range of 2θ angles of 34° to 38°, 44° to 46°, and 64° to 67° were selected, and the Peak FWHM value was converted into radians: β = (FWHM / 180×3.14). The crystal sizes of the three diffraction peaks were calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size of the (Zn, Mg)Al2O4 crystal phase. Wherein, λ is the X-ray wavelength, λ = 0.154056nm, β is the half-peak width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle.

[0187] Crystalline phase content: Import the XRD test results (RAW format) into JADE Standard 8.6 software for fitting and calculation to obtain the content of each crystal phase in the glass ceramic, and then calculate the total content of each crystal phase in the glass ceramic. The ratio of the fitted crystal phase peak area to the fitted total peak area is the crystal phase content of the corresponding crystal phase. The ratio of the fitted crystal phase peak area of ​​the (Zn, Mg)Al2O4 crystal phase to the fitted total peak area is the crystal phase content W of the (Zn, Mg)Al2O4 crystal phase. [(Zn,Mg)Al2O4] The ratio of the peak area of ​​the tetragonal ZrO2 crystal phase to the total peak area of ​​the fitting is the crystal phase content W of the tetragonal ZrO2 crystal phase. [ZrO2] According to W [(Zn,Mg)Al2O4] and W [ZrO2] The ratio (mass ratio Z) of (Zn, Mg)Al2O4 phase and tetragonal ZrO2 phase and the total content W of the crystal phase were calculated.

[0188] Peak intensity ratio: Import the XRD test results (RAW format) into JADE Standard 8.6 software and use the peak search function to determine the 2θ position of the peak and the corresponding raw intensity, and calculate the peak intensity ratio, which is the peak intensity ratio X of the first characteristic peak and the second characteristic peak.

[0189] Half-peak width: Import the XRD test results (RAW format) into JADE Standard 8.6 software for phase retrieval and curve fitting. The 2θ position of the peak and the corresponding crystal plane, half-peak width, and fitting intensity are obtained in the output fitting report. Calculate the ratio based on the fitting intensity of the corresponding crystal plane.

[0190] Specifically, the fitting peak intensity I of the characteristic peak of the

[400] crystal plane

[400] , the fitting peak intensity of the characteristic peak of

[311] crystal plane I

[311] ,

[440] The fitting peak intensity of the characteristic peak of the crystal plane I

[440] , the half-peak width W of the characteristic peak of the

[400] crystal plane

[400] 、The half-peak width W of the characteristic peak of the

[311] crystal plane

[311] 、

[440] half-peak width W of the characteristic peak of the crystal plane

[440] ,I

[400] / I

[311] and I

[440] / I

[311] .

[0191] Taking into account the influence of noise in the test process on peak search, the XRD diffraction peak curve can be smoothed no more than three times.

[0192] 2. Tests of |CT_AV|, DOL_0, CS_50, |CT_CV|

[0193] The stress meter SLP-2000 was used for testing, with a light source wavelength of 518 nm, SOC = 25.5 (nm / cm) / MPa, refractive index = 1.60, and exposure time: 300 usec.

[0194] When testing the surfaces CS_50, |CT_AV|, DOL_0, |CT_CV|, it is necessary to first drop a conductive liquid on the stress meter, then wipe the strengthened spinel glass ceramic sample to be tested clean, place it on the test path, and test its stress value. Among them, the stress meter is SLP-2000 and the conductive liquid used is a conductive liquid with a refractive index of 1.51.

[0195] 3. Thickness test

[0196] The thickness of spinel glass ceramics was tested using a micrometer.

[0197] It should be understood that when chemical strengthening treatment is carried out, the degree of ion exchange changes gradually from the surface to the center in the thickness direction of the spinel glass-ceramics, and the overall Na-K and / or Li-Na exchange amount increment (mass) generally does not exceed 1% of the total mass of the sample. Therefore, the expansion effect in the thickness direction is extremely slight, that is, the thickness of the spinel glass-ceramics changes very little before and after chemical strengthening, and it can be approximately considered that the thickness has basically not changed.

[0198] 4. Optical performance test

[0199] The sample to be tested is cleaned in an ultrasonic cleaning machine, and the cleaning conditions include: cleaning time: 10 minutes; cleaning agent used: detergent diluted 10 times; cleaning temperature: 55±10℃; cleaning frequency: 30±10KHZ. Then the transmittance of the sample to be tested at different wavelengths is tested using a haze meter, and the test is carried out with reference to the standard "GB / T 7962.12-2010 Test method for colorless optical glass Part 12: spectral transmittance". The haze meter used in this patent is the Japanese Konica Minolta spectrophotometer CM-3600A. Among them, the sample to be tested is chemically strengthened glass ceramics or strengthened glass ceramics.

[0200] 5. Vickers hardness HV test

[0201] A reinforced spinel glass-ceramic with a clean surface and no visible scratches, pits, cracks or other damage was selected as a sample. A digital display small load Vickers hardness tester VTD405 (Beijing Wowei Technology Co., Ltd.) was used to test the Vickers hardness of the glass-ceramic in accordance with the national standard GB / T37900-2019 "Ultra-thin glass hardness and fracture toughness test method small load Vickers hardness indentation method". The load was 300gf and the load time was 10s. The effectiveness of the indentation was in accordance with the national standard GB / T 16534-2009 "Fine ceramic room temperature hardness test method". When the Vickers hardness test was performed in this application, a glass-ceramic sample with a length, width and thickness of 50mm×50mm×0.7mm was tested. Three different locations on the same sample surface were selected for measurement, and the average value was selected as the final test result.

[0202] 6. Test of surface K2O concentration

[0203] In the present application, the surface K2O concentration of the strengthened spinel glass ceramics is measured by an X-ray fluorescence spectrometer (XRF), the equipment model used is (Thermo Scientific ARL PERFORM'X), the target material is Rh (rhodium), the light tube voltage is 40kW, the current is 60mA, the collimator is 0.15, the crystal is LiF200, the detector is FPC, the test range is 29mm circle, the analysis software is UniQuant standardless analysis, and the test method adopts the X_UQ method in the OXSAS analysis software. Specifically, the K element content on the surface of the strengthened glass ceramics is measured by an X-ray fluorescence spectrometer (XRF), and then the surface K2O concentration is calculated, and the calculation method is: surface K2O concentration = (surface K element content × relative molecular mass of K2O) / (relative atomic mass of K element × 2). It should be understood that the surface K element content = K element mass / total element mass, and the total element mass = total oxide mass.

[0204] K2O concentration on the surface of strengthened spinel glass-ceramics = K2O mass / total oxide mass, where oxides include SiO2, Al2O3, ZrO2, Na2O, K2O and other oxides that can be accurately tested by XRF, and do not include B2O3 and other oxides that cannot be accurately tested by XRF. XRF testing uses a non-standard test, and does not test the concentration of elements or their oxides with atomic numbers 6 and below in strengthened spinel glass-ceramics. That is, when XRF tests the K2O concentration on the surface of strengthened spinel glass-ceramics, the total oxide mass measured does not include the mass of elements or their oxides with atomic numbers 6 and below in strengthened spinel glass-ceramics.

[0205] 7. Average sandpaper drop resistance test

[0206] The average sandpaper drop height refers to the sum of the sandpaper drop heights measured for each sample of the same embodiment or the same comparative example, and the ratio of the number of reinforced spinel glass-ceramic samples to the number of reinforced spinel glass-ceramic samples, which can be used to characterize the drop damage resistance of the reinforced spinel glass-ceramic. Ten pieces of the same reinforced spinel glass-ceramic samples were taken from each batch for testing, and the average sandpaper drop height was:

[0207]

[0208] Where n is the number of reinforced spinel glass-ceramics samples tested in each batch, and hi is the sandpaper drop resistance height of a single sample tested.

[0209] Among them, the test method for the sandpaper drop height of a single sample is:

[0210] Step 1: Paste 80-grit sandpaper on the lower surface of the 160g model machine, and place the model machine on the green figure LT-SKDL-CD drop machine;

[0211] Step 2: Place a strengthened spinel glass-ceramic sample to be tested with a length, width and thickness of 50mm×50mm×0.7mm directly under the model machine, with the strengthened spinel glass-ceramic sample facing the sandpaper. Make the model machine fall from a certain drop height to impact the strengthened spinel glass-ceramic sample directly under the model machine. If the strengthened spinel glass-ceramic sample does not break, the drop height of the model machine is increased according to a certain rule. For example, the drop height starts from 0.4m, and the sample is dropped once. If it does not break, increase the height by 0.1m each time and drop it again until the strengthened spinel glass-ceramic sample is broken;

[0212] Step 3: The last drop height of the reinforced spinel glass-ceramic sample when it is broken is recorded as the anti-sandpaper drop height. For example, if the drop height when it is broken is 0.5m, the anti-sandpaper drop height of the sample is 0.4m.

[0213] 8. Density

[0214] This application uses the electronic density balance SD-200L of Japan ALFA MIRAGE to test the density of the reinforced spinel. The test principle is the "Archimedes drainage method".

[0215] 9. Fracture toughness test

[0216] The test is carried out according to the national standard GB / T 37900-2019 "Ultra-thin glass hardness and fracture toughness test method - small load Vickers hardness indentation method". Specifically, the indentation is prepared in the same way as the Vickers hardness measurement, and the crack lengths 2C1 and 2C2 in the diagonal direction of the indentation are measured, and their maximum values ​​cannot exceed the thickness of the reinforced spinel glass ceramics. At least 5 effective indentation morphologies are measured on the surface of one sample, and the average value is calculated as the final result value of the sample.

[0217] Indentation fracture toughness calculation formula:

[0218] IFR: Indentation fracture toughness, unit is MPa·m 1 / 2) ; E: elastic modulus of the specimen, in GPa; 2C1, 2C2: crack extension length in the diagonal direction of the indentation, in millimeter (mm); d1, d2: diagonal length of the indentation, in millimeter (mm); F: test load value, in Newton (N).

[0219] In the above test method, the reinforced spinel glass-ceramic tiles in the embodiments and comparative examples are shaped, cut and polished to obtain reinforced spinel glass-ceramic samples of desired size (e.g., polished sheets), which are then tested, such as glass-ceramic polished sheets with a length, width and thickness of 50 mm × 50 mm × 0.7 mm.

[0220] 10. Single rod static pressure strength test

[0221] like Fig.12 As shown, a round glass ceramic sample 10 to be tested with a diameter of 46 mm and a thickness of 0.7 mm is placed on a custom fixture 20 (such as Fig.13 and Fig.14 The glass ceramic sample 10 to be tested is placed in a sample groove 21 of the tensile testing machine (as shown), and then placed on the bottom ring (not shown in the figure) of the tensile testing machine (LT-850A), the test software is started, and the moving speed of the extrusion rod 30 (rod diameter 10mm, ball head diameter 10mm) is set to 10mm / min. Click to start the test, and the extrusion rod 30 will apply force to the center of the glass ceramic sample 10 to be tested at the set moving speed until the glass ceramic sample 10 to be tested is broken.

[0222] The test software will automatically read the force (N) when the glass ceramic sample is broken and record it as the test result. Take 10 glass ceramic samples in the same state for testing, take the average value of the test results, and record it as the single rod static pressure strength that the glass ceramic sample to be tested can withstand.

[0223] The custom fixture in this test method is a cylindrical fixture with a diameter of 65 mm and a height of 20 mm. The specific structure of the custom fixture is as follows: Fig.13 and Fig.14 , where Φ1=65mm, Φ2=46.02mm, Φ3=44mm, h1=20mm, h2=thickness of the reinforced glass ceramic sample to be tested, and h3=15mm. The height of the sample placement groove 21 in the fixture is equal to the thickness of the reinforced glass ceramic sample to be tested, and the reinforced glass ceramic sample to be tested can just be placed in the fixture. The stepped blind hole set in the custom fixture for placing the sample for testing is coaxial with the custom fixture. The fixture is made of acrylic.

[0224] Example 1

[0225] <Preparation of substrate glass>

[0226] According to the formula 1 in Table 1, the raw material formula for glass production was converted into the raw material formula for batching. The total mass of the raw materials was 1000 g, and then mixed with a V-type mixer for 30 minutes. After mixing, 5 g of clarifier NaCl was added, and then transferred to a platinum crucible and melted in a 1650°C lifting furnace (lifting furnace model: SJF1750, manufacturer: Nanjing Boyuntong Instrument Technology Co., Ltd.) for 5 hours, and then poured into a stainless steel mold preheated at 300°C for molding and cooling. It was cooled to 900°C and then placed in a 600°C annealing furnace for annealing for 24 hours. Then it was cooled to room temperature with the furnace to obtain spinel glass ceramics, that is, substrate glass.

[0227] <Preparation of spinel glass ceramics>

[0228] The substrate glass prepared as above was heat-treated in a resistance furnace (equipment model: SLX1400-40, manufacturer: Shanghai Shengli Testing Instrument Co., Ltd.) to obtain spinel glass ceramics.

[0229] Specifically, the two-step heat treatment process is adopted, firstly the temperature is raised to the nucleation temperature for nucleation treatment, and then the temperature is raised to the crystallization temperature for crystallization treatment; the heating rate during the nucleation treatment and crystallization process is 10K / min. Among them, the nucleation temperature T1 is 740℃, the nucleation time t1 is 480min; the crystallization temperature T2 is 800℃, and the crystallization time t2 is 10min.

[0230] According to the needs, the spinel glass ceramics are cut, CNC machined (computer numerical control, i.e., numerical control machine tools, the CNC equipment model used in this application is: RCG500S), and polished in sequence to obtain smooth spinel glass ceramic sheets of the required specifications. In this application, the specifications of the processed spinel glass ceramic sheets are samples with a length, width, and thickness of 50mm×50mm×0.7mm, and circular samples with a diameter of 46mm and a thickness of 0.7mm.

[0231] <Preparation of Strengthened Spinel Glass-Ceramics>

[0232] The spinel glass ceramics were placed in a 100wt% NaNO3 salt bath at 450°C for a first step of strengthening treatment for 3 hours, and then placed in a 100wt% KNO3 salt bath at 430°C for a second step of strengthening treatment for 2 hours to obtain strengthened spinel glass ceramics.

[0233] Example 2 to Example 11

[0234] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1. The corresponding formula in Table 2 is shown in Table 1.

[0235] Example 12 to Example 14

[0236] The method is the same as Example 1 except that the corresponding spinel glass ceramics are placed in a 100 wt % NaNO 3 salt bath at 450° C. for 4 h to obtain the corresponding strengthened spinel glass ceramics as shown in Table 5.

[0237] Example 15 to Example 17

[0238] The method is the same as Example 1 except that the corresponding spinel glass ceramics are placed in a 100wt% KNO3 salt bath at 430°C for 4h to obtain the corresponding strengthened spinel glass ceramics according to Table 6.

[0239] Comparative Example 1 to Comparative Example 11

[0240] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1. The corresponding formula in Table 2 is shown in Table 1.

[0241] Comparative Example 12 to Comparative Example 15

[0242] The method is the same as Example 1 except that the corresponding spinel glass ceramics are placed in a 100 wt % NaNO 3 salt bath at 450° C. for 4 h to obtain the corresponding strengthened spinel glass ceramics as shown in Table 5.

[0243] Comparative Example 16 to Comparative Example 19

[0244] The method is the same as Example 1 except that the corresponding spinel glass ceramics are placed in a 100wt% KNO3 salt bath at 430°C for 4h to obtain the corresponding strengthened spinel glass ceramics according to Table 6.

[0245] The formulations of the embodiments and comparative examples are shown in Table 1, and the preparation parameters and performance tests of the embodiments and comparative examples are shown in Tables 2 to 6.

[0246]

[0247]

[0248]

[0249]

[0250]

[0251] After testing, the spinel glass ceramics of Examples 1 to 11 and Comparative Examples 1 to 11 all contain a main crystalline phase (Zn, Mg) Al2O4 crystalline phase and a secondary crystalline phase tetragonal ZrO2 crystalline phase. The XRD patterns of some Examples and Comparative Examples are shown in FIG. Figures 2 to 7 , Fig. 9, Fig.11 shown.

[0252] Referring to Tables 1 to 4, the composition and structure of the spinel glass ceramics of Examples 1 to 11 are all within the scope of the technical solution of the present application, while the composition and structure of the spinel glass ceramics in Comparative Examples 1 to 11 do not fully meet the requirements of the solution of the present application. By chemically strengthening the spinel glass ceramics in the examples of the present application, a stress level significantly better than that of the comparative example can be obtained. For example, the spinel glass ceramics of the present application can be chemically strengthened to obtain chemically strengthened spinel glass ceramics having a higher compressive stress layer depth and a larger CT. According to tests, the chemically strengthened spinel glass ceramics obtained by chemically strengthening the spinel glass ceramics of the present application have better resistance to drop damage, can withstand higher single-rod static pressure strength, better anti-extrusion performance, higher mechanical strength, and excellent light transmittance. Specifically, Figure 8 As shown, the transmittance of the spinel glass ceramics in Example 1 to visible light is above 80.00%, so that the obtained strengthened spinel glass ceramics are transparent in the visible light range.

[0253] Examples 1 to 3 and Comparative Examples 6 to 9 are all obtained by subjecting the substrate glass of the composition of Formula 1 to different heat treatment systems to obtain spinel glass ceramics, and their XRD diffraction patterns are as follows: Figure 2 shown.

[0254] Reference Figure 2 , Figure 5 As shown in Table 3, the XRD spectrum of the spinel glass ceramic of Example 1 has a first characteristic peak with a 2θ angle in the range of 28° to 32° and a second characteristic peak with a 2θ angle in the range of 36° to 38°, and the peak intensity ratio X is 1.05. Figure 2 As shown in Table 3, the XRD spectrum of the spinel glass ceramics in Comparative Example 6 does not contain a second characteristic peak with a 2θ angle in the range of 36° to 38°, so it does not have a peak intensity ratio X. The (Zn, Mg)Al2O4 crystal phase content in the spinel glass ceramics in Comparative Example 6 is low, and the calculation result of Formula C does not meet the scope of the present application. The stress level of the strengthened spinel glass ceramics obtained in Comparative Example 6 is low. Figure 2 As shown in Table 3, the peak intensity ratio X of the XRD spectrum of the spinel glass ceramic of Comparative Example 7 is 1.61, the (Zn, Mg)Al2O4 crystal phase content in the spinel glass ceramic of Comparative Example 7 is also low, the half-peak width of the characteristic peaks of some crystal planes does not meet the requirements of this application, the calculation result of formula C does not meet the scope of the scheme of this application, and the stress level of the strengthened spinel glass ceramic obtained in Comparative Example 7 is also low. Figure 2 and Figure 4In the XRD spectrum of the spinel glass ceramics of Example 8, the 2θ angle has a peak in the range of 28° to 32°. The content of (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramics of Example 8 is too high, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is too high, and the half-peak width of the characteristic peak of the crystal plane does not meet the requirements of this application. The calculation result of formula C does not meet the scope of the scheme of this application. The stress level of the strengthened spinel glass ceramics prepared in Example 8 is too low. Figure 2 In the XRD spectrum of the spinel glass-ceramics of Comparative Example 9, the 2θ angle shows a peak in the range of 28° to 32°. In the spinel glass-ceramics of Comparative Example 9, the (Zn, Mg)Al2O4 crystal phase content is also relatively high, and the average crystal size of the (Zn, Mg)Al2O4 crystal phase is also relatively high. The calculation result of Formula C does not meet the scope of the present application scheme, and the stress level of the strengthened spinel glass-ceramics obtained in Comparative Example 9 is also relatively low.

[0255] Figure 3 This is a refined diagram of the XRD spectrum of the spinel glass ceramic of Example 6 in the Jade software. In the figure: "XRD original curve" is drawn by the original data obtained by Shimadzu XRD-6100, "fitting curve" is drawn by the fitting data output after curve fitting in Jade software using the RAW file obtained by Shimadzu XRD-6100, "uncertainty curve" is drawn by the difference between the XRD original data and the fitting data output by Jade software, "Zirconium dioxide Bragg position" is the peak position of the zirconium dioxide standard card matched by the XRD original data in Jade, and "Zinc-magnesium spinel Bragg position" is the peak position of the zinc-magnesium spinel standard card matched by the XRD original data in Jade.

[0256] Reference Figure 3 As shown in Table 3, the XRD spectrum of the spinel glass-ceramics of Example 6 has a first characteristic peak with a 2θ angle in the range of 28° to 32° and a second characteristic peak with a 2θ angle in the range of 36° to 38°, and the peak intensity ratio X is 0.97.

[0257] Comparative Examples 10 and 11 are both obtained by using different heat treatment systems on the substrate glass of the composition of Formula 3 to obtain spinel glass ceramics, and their XRD diffraction patterns are as follows: Figure 6 and Figure 7 shown.

[0258] The XRD pattern of the spinel glass ceramic of Comparative Example 10 is as follows: Figure 6As shown in FIG. 1 , the 2θ angle has a peak in the range of 28° to 32°. In the spinel glass ceramic of Comparative Example 10, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is too high, and the calculation result of Formula C does not meet the scope of the present application. The stress level of the strengthened spinel glass ceramic prepared in Comparative Example 10 is too low. The XRD spectrum of the spinel glass ceramic of Comparative Example 11 is as follows: Figure 7 As shown, the 2θ angle has a peak trend in the range of 28° to 32°, and in the spinel glass ceramics of Example 11, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is also relatively high, the half-width of the characteristic peaks of some crystal planes does not meet the requirements of the present application, and the calculation result of Formula C does not meet the scope of the present application. The stress level of the strengthened spinel glass ceramics obtained in Example 11 is also relatively low.

[0259] Comparative Examples 12 to 15 and Examples 12 to 14 obtain spinel glass ceramics by using different heat treatment systems on the substrate glass of the composition of Formula 1, and the chemically strengthened spinel glass ceramics obtained using the same chemical strengthening treatment conditions. The compressive stress layer depth DOL-0 of Comparative Examples 12 to 15 is significantly lower than that of the embodiment scheme of the present application, and the drop damage resistance height measured under 80-mesh sandpaper conditions is also significantly lower than that of the technical scheme of the present application.

[0260] Comparative Examples 16 to 19 and Examples 15 to 17 obtain spinel glass ceramics by using different heat treatment systems on the substrate glass of the composition of Formula 1, and the chemically strengthened spinel glass ceramics obtained using the same chemical strengthening treatment conditions. The single-rod static pressure strength that the chemically strengthened spinel glass ceramics of Comparative Examples 16 to 19 can withstand is significantly lower than the embodiment scheme of the present application, and the surface K2O content is also significantly lower than the embodiment scheme of the present application.

[0261] It should be noted that, in this article, the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0262] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.

[0263] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A spinel glass ceramic, characterized in that: The spinel glass ceramic comprises, in terms of molar percentage of oxides: SiO2 35.00mol% to 60.00mol%, Al2O3 20.00mol% to 40.00mol%, ZrO2 2.00mol% to 8.00mol%, MgO 3.00mol% to 7.50mol%, ZnO 7.00mol% to 13.00mol%, Na2O 1.00mol% to 10.00mol%, Li2O 2.50mol% to 10.00mol%; The spinel glass ceramic contains 15.00 wt % to 45.00 wt % of the (Zn, Mg)Al2O4 crystal phase in the spinel glass ceramic; Take W [(Zn,Mg)Al2O4] is the weight percentage of (Zn, Mg)Al2O4 phase in the spinel glass ceramic, W [Al2O3] is the weight percentage of Al2O3 in the spinel glass ceramic, W [MgO] is the weight percentage of MgO in the spinel glass ceramic, W [ZnO] is the weight percentage of ZnO in the spinel glass ceramic; A=(1-W [(Zn,Mg)Al2O4] / 2)×W [Al2O3] / 2, B=(1-W [(Zn,Mg)Al2O4] )×(W [MgO] +W [ZnO] ), C=A / B, in the spinel glass-ceramics, 1.50≤C≤1.

85.

2. The spinel glass ceramic according to claim 1, characterized in that In the spinel glass ceramics, the value of A is 10.00% to 25.00%, preferably 14.00% to 25.00%; and / or the value of B is 7.50% to 12.50%, preferably 8.00% to 12.00%.

3. The spinel glass ceramic according to claim 1 or 2, characterized in that: The spinel glass ceramics also contain a tetragonal ZrO2 crystal phase, and the total content of the (Zn, Mg)Al2O4 crystal phase and the tetragonal ZrO2 crystal phase accounts for 25.00% to 70.00% by weight of the spinel glass ceramics, and preferably accounts for 30.00% to 50.00% by weight of the spinel glass ceramics.

4. The spinel glass ceramic according to any one of claims 1 to 3, characterized in that In the spinel glass ceramics, the ratio of (Zn, Mg)Al2O4 crystal phase to tetragonal ZrO2 crystal phase is 1.00 to 18.00, preferably 1.00 to 15.

00.

5. The spinel glass ceramic according to any one of claims 1 to 4, characterized in that In the spinel glass-ceramics, the average crystal size of the (Zn, Mg)Al2O4 crystal phase is 3.0 nm to 10.0 nm, preferably 4.0 nm to 8.0 nm, and more preferably 4.0 nm to 7.5 nm.

6. The spinel glass ceramic according to any one of claims 1 to 5, characterized in that: Calculated by molar percentage of oxides, the composition of the spinel glass ceramic further includes: K2O 0.00mol%-5.00mol%, CaO 0.00mol%-10.00mol%, B2O3 0.00mol%-10.00mol%, BaO 0.00mol%-5.00mol%.

7. The spinel glass ceramic according to any one of claims 1 to 6, characterized in that Calculated by molar percentage of oxides, the composition of the spinel glass ceramic includes: SiO2 35.00mol%~60.00mol%, Al2O3 20.00mol%~40.00mol%, ZrO2 2.00mol%~8.00mol%, MgO 4.00mol%~7.00mol%, ZnO9.00mol%~12.00mol%, Na2O 2.00mol%~10.00mol%, and Li2O 3.00mol%~10.00mol%.

8. The spinel glass ceramic according to any one of claims 1 to 7, characterized in that Calculated by molar percentage of oxides, the composition of the spinel glass ceramic includes: SiO2 35.00mol%~50.00mol%, Al2O3 25.00mol%~35.00mol%, ZrO2 3.00mol%~5.00mol%, MgO 4.00mol%~7.00mol%, ZnO9.00mol%~12.00mol%, Na2O 2.00mol%~10.00mol%, and Li2O 3.00mol%~10.00mol%.

9. The spinel glass ceramic according to any one of claims 1 to 8, characterized in that Calculated by the molar percentage of each oxide in the spinel glass ceramic composition, the composition of the spinel glass ceramic satisfies: 1.30≤ZnO / MgO≤2.50; and / or, 0.05≤Li2O / (Al2O3-(MgO+ZnO)+SiO2)≤0.20; and / or, 0.19≤(Al2O3-(MgO+ZnO)) / SiO2≤0.60; and / or, 0.26≤Na2O / Li2O≤3.

00.

10. The spinel glass ceramic according to any one of claims 1 to 9, characterized in that Calculated by the molar percentage of each oxide in the spinel glass ceramic composition, the composition of the spinel glass ceramic also satisfies: 12.00mol%≤ZnO+MgO≤20.00mol%, preferably, 13.00mol%≤ZnO+MgO≤17.30mol%; and / or, 9.00mol%≤Al2O3-(MgO+ZnO)≤22.00mol%, preferably, 10.00mol%≤Al2O3-(MgO+ZnO)≤20.00mol%; and / or, 5.00 mol%≤Na2O+Li2O≤15.00 mol%, preferably, 6.00 mol%≤Na2O+Li2O≤13.50 mol%.

11. The spinel glass ceramic according to any one of claims 1 to 10, characterized in that The spinel glass ceramic is transparent in the visible light range.

12. The spinel glass ceramic according to any one of claims 1 to 11, characterized in that The transmittance of the spinel glass ceramic with a thickness of 0.7 mm under light with a wavelength of 550 nm is greater than or equal to 85%.

13. The spinel glass ceramic according to any one of claims 1 to 12, characterized in that: In the X-ray diffraction pattern of the spinel glass ceramic, the peak with the maximum peak intensity among the characteristic peaks with a 2θ angle in the range of 28° to 32° is taken as the first characteristic peak, and the peak with the maximum peak intensity among the characteristic peaks with a 2θ angle in the range of 36° to 38° is taken as the second characteristic peak, and the peak intensity ratio X between the first characteristic peak and the second characteristic peak is 0.80 to 1.50, and preferably the peak intensity ratio X is 0.85 to 1.

30.

14. The spinel glass ceramic according to any one of claims 1 to 13, characterized in that In the X-ray diffraction spectrum of the spinel glass-ceramic, the characteristic peak of the [400] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle in the range of 44° to 46°, the characteristic peak of the [311] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle in the range of 34° to 38°, and the characteristic peak of the [440] crystal plane of the (Zn, Mg)Al2O4 crystal phase is located at a 2θ angle in the range of 64° to 67°; The half-peak width W of the characteristic peak of the [400] crystal plane is [400] 0.650°~1.800°, preferably W [400] 0.900° to 1.600°; The half-peak width W of the characteristic peak of the [311] crystal plane is [311] 0.900°~2.800°, preferably W [311] 1.100° to 2.230°; The half-peak width W of the characteristic peak of the [440] crystal plane is [440] 0.750°~2.000°, preferably W [440] 0.900° to 1.600°.

15. A glass device made from the spinel glass ceramic according to any one of claims 1 to 14. 16 . An electronic device comprising the spinel glass ceramic according to claim 1 .

Citation Information

Patent Citations

  • White, opaque, beta-spodumene / rutile glass-ceramics,articles comprising the same,and methods for making the same

    CN104619665A

  • White, opaque, [beta]-spodumene glass-ceramic articles with inherent damage resistance and methods for making the same

    CN106660861A

  • Ion exchangeable, transparent gahnite-spinel glass ceramics with high hardness and modulus

    CN111615500A

  • White, opaque, [beta]-spodumene glass-ceramic articles with inherent damage resistance and methods for making the same

    CN111792848A

  • Ion exchangeable, opaque gahnite-spinel glass ceramics with high hardness and modulus

    CN113365957A

Cited By

  • Spinel glass ceramic and use thereof

    WO2025139527A1