Preparation method of micro-patterned super-hydrophilic self-cleaning composite coating

By depositing Bi2MoO6 on quartz glass and applying a TiO2 coating, combined with deep ultraviolet photodegradation and dissolution, a micro-patterned super-hydrophilic TiO2/Bi2MoO6 composite coating was formed, which solved the problem of photogenerated current carrying in hydrophilic photocatalytic coatings. The problem of fast sub-recombination rate improves the photocatalytic activity and self-cleaning performance and is suitable for industrial production.

CN118754458AInactive Publication Date: 2024-10-11XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410933781.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing hydrophilic photocatalytic coatings have the problem of poor photocatalytic activity due to fast photogenerated carrier recombination rate.

Method used

The Bi2MoO6 coating is deposited on the quartz glass substrate using the sol-gel method, and the TiO2 coating is applied on the Bi2MoO6 coating through the dip pulling method, combined with a mask to assist deep ultraviolet photodegradation and dissolution, to form a micro-patterned Super hydrophilic TiO2/Bi2MoO6 composite coating builds a heterojunction to reduce the recombination rate of photogenerated carriers.

Benefits of technology

It improves the self-cleaning performance, achieves super-hydrophilicity and uniformity, reduces the photogenerated carrier recombination rate of the photocatalytic material, improves the photocatalytic performance, has a simple process and low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754458A_ABST
    Figure CN118754458A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a micro-patterned super-hydrophilic self-cleaning composite coating, which is specifically implemented according to the following steps: step 1, depositing a Bi2MoO6 coating on a quartz glass substrate by adopting a sol-gel method; step 2, coating the Bi2MoO6 coating with a TiO2 coating by adopting a dip-coating method, and then carrying out deep ultraviolet light degradation and dissolving washing under the assistance of a mask plate, so as to obtain a TiO2 coating with a micro-patterned rough structure; and step 3, crystallizing the TiO2 coating through annealing treatment, and cooling along with a furnace to obtain the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating. The micro-patterned super-hydrophilic self-cleaning composite coating prepared by the method disclosed by the invention has excellent hydrophilic property, achieves a super-hydrophilic state, and has the characteristics of good uniformity, no micro-crack, stable performance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of self-cleaning materials, and in particular relates to a method for preparing a micro-patterned super-hydrophilic self-cleaning composite coating. Background Art

[0002] Self-cleaning coatings can effectively treat pollutants on the surface of materials, and have the advantages of environmental protection, energy saving, and low cost. They have gradually become a hot topic in the building materials, new energy, and medical industries. Common self-cleaning coatings are mainly divided into the following three categories: hydrophilic coatings, hydrophobic coatings, and semiconductor photocatalytic coatings. Compared with hydrophobic coatings, hydrophilic coatings have attracted much attention from researchers because of their higher durability. However, the composition of various organic pollutants is complex, and a single hydrophilic coating cannot completely degrade pollutants. Generally, they are combined with semiconductor photocatalytic coatings to utilize the synergistic effect of photocatalytic degradation of organic pollutants and hydrophilic surfaces to improve the self-cleaning effect. However, the existing hydrophilic photocatalytic coatings still have the problem of poor photocatalytic activity due to the fast recombination rate of photogenerated carriers. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a micro-patterned super-hydrophilic self-cleaning composite coating, so as to solve the problem that the existing hydrophilic photocatalytic coating has a fast recombination rate of photogenerated carriers resulting in poor photocatalytic activity.

[0004] The technical solution adopted by the present invention is a method for preparing a micro-patterned super-hydrophilic self-cleaning composite coating, which is specifically implemented according to the following steps:

[0005] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0006] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0007] Step 3, crystallizing the TiO2 coating by annealing, and obtaining a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating by furnace cooling.

[0008] The present invention is also characterized in that:

[0009] The specific process of step 1 is:

[0010] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with 68% by mass of concentrated nitric acid, stir magnetically, add acetylacetone, continue stirring, and stand for aging to obtain Bi2MoO6 coating slurry;

[0011] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method, and then heat-treating the quartz glass with the initial Bi2MoO6 coating and cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating.

[0012] In step 1.1, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate, and acetylacetone is 14:1:7.5-15;

[0013] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20, and the amount of ethylene glycol methyl ether added is such that the total concentration of metal ions is 0.25 mol / L to 0.4 mol / L.

[0014] In step 1.2, the pulling speed of the immersion pulling method is 1.5 mm / s to 3 mm / s;

[0015] The temperature of the heat treatment is 450°C to 550°C, and the time of the heat treatment is 40min to 60min.

[0016] The specific process of step 2 is:

[0017] Step 2.1, adding tetrabutyl titanate and acrylic acid into anhydrous methanol at room temperature, stirring with a magnetic stirrer, and standing for aging to obtain a TiO2 coating slurry;

[0018] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by using an immersion and pulling method;

[0019] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask plate, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern;

[0020] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in a solvent, and then drying it in N2 to obtain a TiO2 coating with a micro-patterned rough structure.

[0021] In step 2.1, the molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is such that the total concentration of metal ions is 0.1 mol / L to 0.5 mol / L.

[0022] In step 2.2, the pulling speed of the immersion pulling method is 1.5 mm / s to 3 mm / s.

[0023] In step 2.3, deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm as an exposure light source, and the irradiation time is 1h to 3h.

[0024] In step 3, the annealing temperature is 450° C. to 500° C., and the holding time is 40 min to 60 min.

[0025] The beneficial effects of the present invention are:

[0026] (1) The micro-patterned super-hydrophilic self-cleaning composite coating prepared by the present invention not only takes into account the respective advantages of TiO2 and Bi2MoO6 materials, but also utilizes the synergistic effect of micro-patterning and two semiconductor heterojunctions to effectively improve the self-cleaning performance;

[0027] (2) The micro-patterned super-hydrophilic self-cleaning composite coating prepared by the present invention has excellent hydrophilic properties and reaches a super-hydrophilic state. It also has the characteristics of good uniformity, no micro-cracks and stable performance, and is expected to be industrialized in the field of self-cleaning;

[0028] (3) The micro-patterned super-hydrophilic self-cleaning composite coating prepared by the present invention adopts a heterojunction modification method to reduce the recombination rate of photogenerated carriers, thereby obtaining excellent self-cleaning performance by improving the photocatalytic performance of both;

[0029] (4) The method for preparing a micro-patterned super-hydrophilic self-cleaning composite coating of the present invention directly prepares a TiO2 micro-pattern on a Bi2MoO6 coating through deep ultraviolet (DUV) light degradation and washing assisted by a mask, thereby realizing the simultaneous preparation of a TiO2 / Bi2MoO6 composite coating and micro-patterning processing. The preparation process does not require expensive equipment, corrosive media, or photoresist, has a simple process flow, and is low in cost, and is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 X-ray diffraction patterns of the Bi2MoO6 coatings prepared in Examples 1 to 3 of the present invention;

[0031] Figure 2 The X-ray diffraction pattern of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in Example 4 of the present invention;

[0032] Figure 3 This is a laser confocal micrograph of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in Example 4 of the present invention;

[0033] Figure 4 This is a hydrophilicity test diagram of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in Example 4 of the present invention;

[0034] Figure 5This is a diagram showing the effect of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in Example 4 of the present invention on the degradation of 5 μL of pollutants under visible light at room temperature. DETAILED DESCRIPTION

[0035] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0036] The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating of the present invention is specifically implemented according to the following steps:

[0037] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0038] The specific process is:

[0039] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with about 68% by mass of concentrated nitric acid, stir magnetically, add acetylacetone, continue stirring, and allow to stand for aging to obtain a Bi2MoO6 coating slurry;

[0040] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate and acetylacetone is 14:1:7.5-15;

[0041] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20, and the amount of ethylene glycol methyl ether added is such that the total concentration of metal ions is 0.25 mol / L to 0.4 mol / L;

[0042] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method, and then heat-treating the quartz glass with the initial Bi2MoO6 coating and cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0043] Among them, the pulling speed of the immersion pulling method is 1.5mm / s to 3mm / s;

[0044] The heat treatment temperature is 450°C to 550°C, and the heat treatment time is 40min to 60min;

[0045] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by a dip-coating method, and then performing deep ultraviolet (DUV) photodegradation and washing with the aid of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0046] The specific process is:

[0047] Step 2.1, adding tetrabutyl titanate and acrylic acid into anhydrous methanol at room temperature, stirring with a magnetic stirrer, and standing for aging to obtain a TiO2 coating slurry;

[0048] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is such that the total concentration of metal ions is 0.1 mol / L to 0.5 mol / L;

[0049] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by using an immersion and pulling method;

[0050] Among them, the pulling speed of the immersion pulling method is 1.5mm / s to 3mm / s;

[0051] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask plate, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern;

[0052] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm as the exposure light source, and the irradiation time is 1h to 3h;

[0053] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in a solvent, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0054] Step 3, crystallizing the TiO2 coating by annealing, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating;

[0055] The annealing temperature is 450°C to 500°C, and the holding time is 40min to 60min.

[0056] The present invention realizes the simultaneous preparation of TiO2 / Bi2MoO6 composite coating and fine patterning processing, wherein in the mask-assisted deep ultraviolet (DUV) light degradation and washing process, no photoresist is needed, the process flow is simple, and the preparation cost is low.

[0057] Since both TiO2 and Bi2MoO6 are hydrophilic, according to the Wenzel wettability principle, constructing a certain rough structure on the surface of a hydrophilic material will increase its hydrophilicity. Therefore, the method of the present invention constructs a TiO2 rough structure on the surface of Bi2MoO6 through micro-patterning, so that the TiO2 / Bi2MoO6 self-cleaning composite coating has super-hydrophilic properties; on the other hand, both TiO2 and Bi2MoO6 are semiconductor photocatalytic materials, and the energy band structures of the two are matched, which facilitates the use of heterojunction modification means to reduce the recombination rate of photogenerated carriers, thereby obtaining excellent self-cleaning performance by improving the photocatalytic performance of the two.

[0058] Example 1

[0059] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0060] The specific process is:

[0061] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid having a mass fraction of about 68%, and add ethylene glycol methyl ether in an amount such that the total concentration of metal ions is 0.4 mol / L, stir magnetically for 2 h, add acetylacetone, continue stirring for 6 h, and allow to stand for at least 12 h to obtain a Bi2MoO6 coating slurry;

[0062] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate and acetylacetone is 14:1:7.5;

[0063] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20;

[0064] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method at a pulling speed of 3 mm / s, and then heat-treating the quartz glass with the initial Bi2MoO6 coating at 450° C. for 40 min and then cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0065] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0066] The specific process is:

[0067] Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred for 2 hours, and allowed to stand for 12 hours to obtain a TiO2 coating slurry;

[0068] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is fixed to a total metal ion concentration of 0.1 mol / L;

[0069] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by an immersion pulling method at a pulling speed of 3 mm / s;

[0070] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern to improve surface roughness;

[0071] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm and a main wavelength of 325nm as the exposure light source, and the irradiation time is 1h;

[0072] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in acetone for 10 seconds, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0073] Step 3, annealing at 450°C for 40 minutes to crystallize the TiO2 coating, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating.

[0074] Example 2

[0075] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0076] The specific process is:

[0077] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid having a mass fraction of about 68%, and add ethylene glycol methyl ether in an amount such that the total metal ion concentration is 0.35 mol / L, stir magnetically for 2 h, add acetylacetone, continue stirring for 6 h, and allow to stand for at least 12 h to obtain a Bi2MoO6 coating slurry;

[0078] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate and acetylacetone is 14:1:10;

[0079] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20;

[0080] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method at a pulling speed of 2 mm / s, and then heat-treating the quartz glass with the initial Bi2MoO6 coating at 500° C. for 50 min and then cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0081] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0082] The specific process is:

[0083] Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred for 2 hours, and allowed to stand for 12 hours to obtain a TiO2 coating slurry;

[0084] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is fixed to a total metal ion concentration of 0.2 mol / L;

[0085] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by an immersion pulling method at a pulling speed of 2 mm / s;

[0086] Step 2.3, depositing the TiO2 coating applied in step 2.2 by deep ultraviolet radiation, and then covering the deposited TiO2 coating with a mask having a size of 3 μm, and continuing to irradiate to obtain a TiO2 coating with an array pattern, thereby improving the surface roughness;

[0087] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm and a main wavelength of 325nm as the exposure light source, and the irradiation time is 2h;

[0088] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in acetone for 8 seconds, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0089] Step 3, annealing at 500°C for 50 minutes to crystallize the TiO2 coating, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating.

[0090] Example 3

[0091] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0092] The specific process is:

[0093] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid having a mass fraction of about 68%, and add ethylene glycol methyl ether in an amount such that the total concentration of metal ions is 0.3 mol / L, stir magnetically for 2 h, add acetylacetone, continue stirring for 6 h, and allow to stand for at least 12 h to obtain a Bi2MoO6 coating slurry;

[0094] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate, and acetylacetone is 14:1:12.5;

[0095] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20;

[0096] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method at a pulling speed of 2 mm / s, and then heat-treating the quartz glass with the initial Bi2MoO6 coating at 550° C. for 60 min and then cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0097] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0098] The specific process is:

[0099] Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred for 2 hours, and allowed to stand for 12 hours to obtain a TiO2 coating slurry;

[0100] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is such that the total concentration of metal ions is 0.3 mol / L;

[0101] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by an immersion pulling method at a pulling speed of 2 mm / s;

[0102] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern to improve surface roughness;

[0103] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm and a main wavelength of 325nm as the exposure light source, and the irradiation time is 3h;

[0104] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in acetone for 7 seconds, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0105] Step 3, annealing at 500°C for 60 minutes to crystallize the TiO2 coating, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating.

[0106] like Figure 1 As shown, it is the X-ray diffraction spectrum of the Bi2MoO6 coating prepared in Examples 1 to 3. It can be seen from the figure that the bismuth molybdate coating prepared in Examples 1 to 3 has no impurity phase and good crystallinity.

[0107] Example 4

[0108] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0109] The specific process is:

[0110] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid having a mass fraction of about 68%, and add ethylene glycol methyl ether in an amount such that the total metal ion concentration is 0.25 mol / L, stir magnetically for 2 h, add acetylacetone, continue stirring for 6 h, and allow to stand for at least 12 h to obtain a Bi2MoO6 coating slurry;

[0111] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate and acetylacetone is 14:1:15;

[0112] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20;

[0113] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method at a pulling speed of 1.5 mm / s, and then heat-treating the quartz glass with the initial Bi2MoO6 coating at 550° C. for 60 min and then cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0114] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0115] The specific process is:

[0116] Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred for 2 hours, and allowed to stand for 12 hours to obtain a TiO2 coating slurry;

[0117] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is fixed to a total metal ion concentration of 0.4 mol / L;

[0118] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by an immersion pulling method at a pulling speed of 1.5 mm / s;

[0119] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern to improve surface roughness;

[0120] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm and a main wavelength of 325nm as the exposure light source, and the irradiation time is 2h;

[0121] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in acetone for 8 seconds, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0122] Step 3, annealing at 500°C for 60 minutes to crystallize the TiO2 coating, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating.

[0123] like Figure 2 As shown, it is the X-ray diffraction spectrum of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in this embodiment. The analysis shows that the prepared super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating has no impurities and good crystallinity.

[0124] like Figure 3 As shown, it is a laser confocal micrograph of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in this embodiment. It can be clearly observed that the array structure with a certain degree of roughness exists on the surface.

[0125] like Figure 4 As shown, the hydrophilicity test of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in this embodiment shows that its water contact angle is only 4°, reaching a super-hydrophilic state.

[0126] like Figure 5 As shown, the self-cleaning performance test of the super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating prepared in this embodiment, 5 μL of pollutants were completely removed after 12 minutes.

[0127] Example 5

[0128] Step 1, depositing a Bi2MoO6 coating on a quartz glass substrate using a sol-gel method;

[0129] The specific process is:

[0130] Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid having a mass fraction of about 68%, and add ethylene glycol methyl ether in an amount such that the total concentration of metal ions is 0.4 mol / L, stir magnetically for 2 h, add acetylacetone, continue stirring for 6 h, and allow to stand for at least 12 h to obtain a Bi2MoO6 coating slurry;

[0131] Wherein, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate, and acetylacetone is 14:1:7.5;

[0132] The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20;

[0133] Step 1.2, immersing the quartz glass into the Bi2MoO6 coating slurry obtained in step 1.1, preparing an initial Bi2MoO6 coating on the quartz glass by an immersion pulling method at a pulling speed of 3 mm / s, and then heat-treating the quartz glass with the initial Bi2MoO6 coating at 450° C. for 40 min and then cooling it to room temperature with the furnace to obtain a Bi2MoO6 coating;

[0134] Step 2, coating a TiO2 coating on the Bi2MoO6 coating by an immersion-coating method, and then degrading and washing with deep ultraviolet light with the assistance of a mask to obtain a TiO2 coating with a micro-patterned rough structure;

[0135] The specific process is:

[0136] Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred for 2 hours, and allowed to stand for 12 hours to obtain a TiO2 coating slurry;

[0137] The molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is such that the total concentration of metal ions is 0.5 mol / L;

[0138] Step 2.2, immersing the Bi2MoO6 coating obtained in step 1 into the TiO2 coating slurry obtained in step 2.1, and coating the TiO2 coating on the Bi2MoO6 coating by an immersion pulling method at a pulling speed of 3 mm / s;

[0139] Step 2.3, placing the TiO2 coating applied in step 2.2 under a mask plate, and applying deep ultraviolet radiation to obtain a TiO2 coating with an array pattern to improve the surface roughness;

[0140] Deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm and a main wavelength of 325nm as the exposure light source, and the irradiation time is 1h;

[0141] Step 2.4, washing the TiO2 coating with the array pattern obtained in step 2.3 in acetone for 10 seconds, and then drying in N2 to obtain a TiO2 coating with a micro-patterned rough structure;

[0142] Step 3, annealing at 480°C for 40 minutes to crystallize the TiO2 coating, and cooling in the furnace to obtain a super-hydrophilic micro-patterned TiO2 / Bi2MoO6 self-cleaning composite coating.

Claims

1. Preparation method of micro-patterned super-hydrophilic self-cleaning composite coating, It is characterized in that Follow the steps below to implement it: Step 1: Deposit Bi on a quartz glass substrate using a sol-gel method. 2 MoO 6 coating; Step 2: Using the immersion pulling method to 2 MoO 6 TiO coating 2 The coating is then degraded and washed with deep ultraviolet light assisted by a mask to obtain a TiO 2 coating; Step 3: annealing TiO 2 The coating crystallizes and cools in the furnace to obtain super-hydrophilic micro-patterned TiO 2 / Bi 2 MoO 6 Self-cleaning composite coating.

2. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 1, It is characterized in that The specific process of step 1 is: Step 1.1, at room temperature, add bismuth nitrate pentahydrate and ammonium heptamolybdate tetrahydrate to ethylene glycol methyl ether acidified with concentrated nitric acid, stir magnetically, add acetylacetone, continue stirring, and allow to stand for aging to obtain Bi 2 MoO 6 Coating slurry; Step 1.2, immerse the quartz glass into the Bi obtained in step 1.1 2 MoO 6 In the coating slurry, the initial Bi was prepared on quartz glass by immersion pulling method. 2 MoO 6 coating, and then the initial Bi 2 MoO 6 After the coated quartz glass is heat treated, it is cooled to room temperature in the furnace to obtain Bi 2 MoO 6 coating.

3. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 2, It is characterized in that In step 1.1, the molar ratio of bismuth nitrate pentahydrate, ammonium heptamolybdate tetrahydrate, and acetylacetone is 14:1:7.5-15; The molar ratio of nitric acid to ethylene glycol methyl ether is 1:20, and the amount of ethylene glycol methyl ether added is such that the total concentration of metal ions is 0.25 mol / L to 0.4 mol / L.

4. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 2, It is characterized in that In step 1.2, the pulling speed of the immersion pulling method is 1.5 mm / s to 3 mm / s; The temperature of the heat treatment is 450°C to 550°C, and the time of the heat treatment is 40min to 60min.

5. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 1, It is characterized in that The specific process of step 2 is: Step 2.1, at room temperature, tetrabutyl titanate and acrylic acid are added to anhydrous methanol, magnetically stirred, and allowed to stand for aging to obtain TiO 2 Coating slurry; Step 2.2: Bi obtained in step 1 2 MoO 6 The TiO coating obtained in step 2.1 was immersed in 2 In the coating slurry, the Bi 2 MoO 6 TiO coating 2 coating; Step 2.3: Apply the TiO coated in step 2.2 2 The coating is placed under a mask and irradiated with deep ultraviolet light to obtain a TiO 2 coating; Step 2.4: Place the TiO2 with array pattern obtained in step 2.3 2 After the coating is dissolved in a solvent, it is then 2 After drying, TiO with micro-patterned rough structure was obtained. 2 coating.

6. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 5, It is characterized in that In step 2.1, the molar ratio of tetrabutyl titanate to acrylic acid is 1:3; the amount of anhydrous methanol added is such that the total concentration of metal ions is 0.1 mol / L to 0.5 mol / L.

7. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 5, It is characterized in that In step 2.2, the pulling speed of the immersion pulling method is 1.5 mm / s to 3 mm / s.

8. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 5, It is characterized in that In step 2.3, deep ultraviolet irradiation uses a deep ultraviolet lamp with a wavelength of 200nm to 350nm as an exposure light source, and the irradiation time is 1h to 3h.

9. The method for preparing the micro-patterned super-hydrophilic self-cleaning composite coating according to claim 1, It is characterized in that In step 3, the annealing temperature is 450° C. to 500° C., and the holding time is 40 min to 60 min.