Steel slag harmless treatment method, harmless steel slag and application of harmless steel slag
By grinding steel slag together with aluminum sulfate-based materials and alum-based materials, ettringite and hydrotalcite are generated, which solves the problem of poor stability of cement-based materials caused by free calcium oxide and magnesium oxide in steel slag, and realizes the harmlessness of steel slag Processing and efficient resource utilization significantly reduce processing costs and energy consumption.
Patent Information
- Application Number
- CN202410823561.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
AI Technical Summary
The high content of free calcium oxide and free magnesium oxide in steel slag leads to poor stability of cement-based materials. The existing treatment methods are time-consuming, energy-intensive and costly, making it difficult to effectively utilize steel slag as a resource.
Grinding steel slag with aluminum sulfate-based materials and alum-based materials together produces ettringite and hydrotalcite, consuming low active oxides, improving reaction speed and grinding efficiency, reducing free calcium oxide and magnesium oxide content, and meeting national standards.
It achieves harmless treatment of steel slag, reduces the stability risk of cement-based materials, and improves the utilization rate of steel slag in building materials manufacturing. It has a simple process, low energy consumption and low cost.
Smart Images

Figure BDA0004909791780000041 
Figure BDA0004909791780000051 
Figure BDA0004909791780000052
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of inorganic building materials, and specifically relates to a harmless treatment method for solid waste, and in particular to a harmless treatment method for steel slag, steel slag that is harmless to building materials, and application of the steel slag in building material manufacturing. Background Art
[0002] Steel slag is an industrial waste produced during the steelmaking process, accounting for about 15% of crude steel production. The utilization rate of steel slag is low, only about 30%. According to statistics, the accumulated stock of steel slag in my country currently exceeds 1.8 billion tons. The long-term storage of steel slag not only wastes resources, but also easily generates dust, causing pollution to nearby waters, thus causing a series of environmental problems.
[0003] The preparation of building materials is the main way to recycle solid waste, but it is very difficult to use steel slag in cement-based materials. The main reason is that steel slag contains a large amount of oxides such as free calcium oxide and free magnesium oxide. Affected by factors such as smelting process, the free calcium oxide content in steel slag can reach 1% to 20%, and the free magnesium oxide content is usually 3% to 10%. These oxides are formed by high-temperature calcination (about 1600°C) and have low activity. When added to cement, they will cause poor stability problems in cement-based materials and seriously affect component performance and structural safety. The national standard GB / T 20491-2017 "Steel Slag Powder for Cement and Concrete" clearly stipulates that the free calcium oxide content in steel slag powder shall not exceed 4%, and when the magnesium oxide content exceeds 5%, stability testing is required. Therefore, the harmless treatment of free calcium oxide and free magnesium oxide in steel slag and solving the poor stability problems brought to cement-based materials are the key technical bottlenecks to promote the resource utilization of steel slag.
[0004] In the prior art, natural aging, water immersion, steam treatment, ultrafine grinding, heat treatment, etc. are usually used to treat steel slag harmlessly. The natural aging method takes a long time, usually several months or even years; the water immersion method consumes a lot of water resources; the steam treatment method requires complex equipment and consumes a certain amount of energy; the ultrafine grinding method and heat treatment method have high energy consumption.
[0005] Therefore, it is necessary to develop a simple, easy and efficient harmless treatment method to effectively remove low-activity oxides in steel slag. Summary of the invention
[0006] In view of the above background, the primary purpose of the present invention is to provide a method for harmless treatment of steel slag, which can effectively remove low-activity oxides such as free calcium oxide and free magnesium oxide contained in the steel slag, so as to reduce the risk of adverse stability of cement-based building materials caused by steel slag and improve the utilization rate of steel slag in the manufacture of building materials.
[0007] Another object of the present invention is to provide steel slag obtained by the harmless treatment method, and its application in the preparation of building materials.
[0008] The above-mentioned purpose of the present invention is achieved by the following method:
[0009] In a first aspect, the present invention provides a method for harmless treatment of steel slag, which comprises grinding the steel slag and aluminum sulfate materials and / or alum materials together to a specific surface area of not less than 200 m 2 / kg.
[0010] In the scheme described in the present invention, the steel slag refers to a by-product composed of various oxides formed by oxidation of impurities such as silicon, manganese, phosphorus, sulfur, etc. in pig iron during high-temperature (about 1600°C) smelting, as well as salts generated by the reaction of these oxides with solvents; wherein the content of free calcium oxide and free magnesium oxide is usually between 1% and 20%.
[0011] In the solution of the present invention, the sum of the mass of the aluminum sulfate material and the alum material accounts for no less than 1% of the mass of the steel slag. In a preferred solution, the sum of the mass of the aluminum sulfate material and the alum material accounts for 2% to 20% of the mass of the steel slag; more preferably 4% to 15%; further preferably 4% to 10%; most preferably 7% to 10%.
[0012] In a preferred embodiment of the present invention, the aluminum sulfate material is a combination of one or more of industrial aluminum sulfate, aluminum sulfate 18hydrate, aluminum sulfate 16hydrate, and anhydrous aluminum sulfate. In a further preferred embodiment, the aluminum sulfate material is aluminum sulfate 16hydrate or aluminum sulfate 18hydrate; aluminum sulfate 18hydrate is most preferred.
[0013] In a preferred embodiment of the present invention, the alum material is a combination of one or more of potassium aluminum sulfate dodecahydrate, sodium aluminum sulfate dodecahydrate, and ammonium aluminum sulfate dodecahydrate. In a further preferred embodiment, the alum material is sodium aluminum sulfate dodecahydrate or potassium aluminum sulfate dodecahydrate; potassium aluminum sulfate dodecahydrate is most preferred.
[0014] In a preferred embodiment of the present invention, a grinding aid may be added during the grinding process. The grinding aid may be selected from any one or a combination of at least two of triethanolamine, ethylene glycol, propylene glycol, sodium sulfate, gypsum, fatty acids and their salts, phosphates, glycerol or polycarboxylates.
[0015] In the preferred embodiment of the present invention, the co-grinding is grinding to a specific surface area of 200m 2 / kg~1000m 2 / kg; more preferably 400m 2 / kg~800m 2 / kg; 400m3 is the most preferred 2 / kg.
[0016] In a second aspect, the present invention provides a steel slag that is harmless to building materials, which is obtained by the harmless treatment method described in the first aspect of the present invention; the free calcium oxide content in the steel slag that is harmless to building materials is not higher than 3%, and the free magnesium oxide content is not higher than 1.5%, which meets the requirements of the national standard GB / T 20491-2017 "Steel slag powder used in cement and concrete" that the free calcium oxide content is not higher than 4%, and the magnesium oxide content is not higher than 5%.
[0017] In a third aspect, the present invention further provides the use of the steel slag harmless to building materials described in the second aspect of the present invention in the preparation of building materials.
[0018] The application includes using the steel slag which is harmless to building materials and mixing it with cement to produce cement-based materials.
[0019] In a preferred application of the present invention, the mass ratio of the steel slag harmless to building materials to cement is no higher than 2:1; more preferably 0.1 to 1.5:1; further preferably 0.5 to 1.5:1; further preferably 0.5 to 1.0:1; and most preferably 0.5:1.
[0020] In a preferred application of the present invention, the cement is one of silicate cement and sulphoaluminate cement.
[0021] The mechanism of harmless treatment of steel slag described in the present invention mainly lies in the following points:
[0022] 1. When steel slag is ground together with aluminum sulfate and alum materials, the effective ingredients of aluminum sulfate and potassium aluminum sulfate in aluminum sulfate and alum materials are acidic substances, which can react quickly with the low-activity free calcium oxide and free magnesium oxide in the steel slag to generate ettringite and hydrotalcite respectively, consuming the above-mentioned alkaline oxides, thereby avoiding the poor stability problems caused by them. The reaction equation is as follows:
[0023] Al 2 (SO 4 ) 3 18H 2 O+6CaO+14H 2 O=3CaO·Al 2 O 3 ·3CaSO 4 ·32H 2 O
[0024] Al 2 (SO 4 ) 3 18H 2 O + 7MgO = 3MgSO 4 +Mg 4 Al2 (OH) 10 +8H 2 O
[0025] 2. The present invention grinds steel slag together with aluminum sulfate materials and alum materials, so that the steel slag can be fully contacted with aluminum sulfate materials and alum materials, thereby improving the above reaction speed and degree, thereby ensuring the efficiency of eliminating alkaline oxides and reducing the chemical reaction time required for harmless treatment.
[0026] 3. In the harmless treatment method of the present invention, aluminum sulfate materials and alum materials can simultaneously play a grinding aid role, which can improve the grinding efficiency of steel slag.
[0027] In summary, compared with existing treatment methods, the harmless treatment method of the present invention has the advantages of simple process, low energy consumption and low cost. DETAILED DESCRIPTION
[0028] The scheme and technical effects of the present invention are further described in detail below by listing examples and comparative examples. However, the examples listed should not be construed as limiting the scheme of the present invention.
[0029] Example 1-Example 15
[0030] Steel slag from Hesteel Group was taken for harmless treatment, which contained 9% free calcium oxide and 5% free magnesium oxide. As listed in Table 1, the steel slag was mixed with aluminum sulfate 18hydrate and / or potassium aluminum sulfate 12hydrate, and ground together to a certain specific surface area, and then the residual free calcium oxide content and residual free magnesium oxide content in the steel slag were measured. The measurement results are shown in Table 1.
[0031] Table 1.
[0032]
[0033] As shown in Table 1, 1-15 parts of aluminum sulfate 18hydrate are added to every 100 parts of steel slag and ground to 400 m 2 / kg, can achieve the harmless treatment of steel slag, obtain steel slag with very low residual free calcium oxide and free magnesium oxide, and significantly reduce the risk of affecting the stability of building materials. It can be seen from the above examples 1-6 that in the process of increasing the addition amount of aluminum sulfate 18hydrate from 1 part to 10 parts, the residual amount of free calcium oxide and free magnesium oxide will continue to decrease, but when the addition amount of aluminum sulfate 18hydrate reaches 10 parts, the residual amount of free calcium oxide and free magnesium oxide is reduced to the minimum, and adding more aluminum sulfate 18hydrate will not bring about a further decrease in the residual amount of free calcium oxide and free magnesium oxide. In addition, when the 2 parts of aluminum sulfate 18hydrate added in Example 2 are replaced with potassium aluminum sulfate 12hydrate (Example 7) or when 2 parts of the 4 parts of aluminum sulfate 18hydrate added in Example 3 are replaced with potassium aluminum sulfate 12hydrate (Example 8), the effect before and after the replacement is equivalent. It can be seen from the above examples 9-15 that the residual amount of free calcium oxide and free magnesium oxide will decrease within a certain range as the fineness of the co-grinding increases, but grinding to 400m 2 / kg, the residual amount of free calcium oxide and free magnesium oxide will not decrease further with the increase of grinding fineness.
[0034] Comparative Example 1-Comparative Example 4
[0035] The same steel slag as in Example 1 to Example 15 was treated for harmlessness. As shown in Table 2, the steel slag was mixed with aluminum sulfate 18hydrate or potassium aluminum sulfate 12hydrate, and ground together to a certain specific surface area, and then the residual free calcium oxide content and the residual free magnesium oxide content in the steel slag were measured. The measurement results are shown in Table 2.
[0036] Table 2.
[0037]
[0038] As shown in Table 2, compared with Examples 1-7, although Comparative Examples 1-3 were all ground to 400 m 2 / kg, but when aluminum sulfate 18hydrate or aluminum potassium sulfate 12hydrate is not added or the addition amount is too small, the harmless treatment of steel slag cannot be effectively achieved, and the residual amount of free calcium oxide and free magnesium oxide in the treated steel slag is still high (the free calcium oxide content is higher than 3%, and the free magnesium oxide content is higher than 1.8%), which will still have an adverse effect on the stability of building materials. In addition, it can be seen from Comparative Example 4 that compared with Example 3, although an equal amount of aluminum sulfate 18hydrate is added, the fineness of the co-grinding is insufficient, and the reaction of aluminum sulfate with free calcium oxide or free magnesium oxide in the steel slag is insufficient, resulting in a high residual amount of free calcium oxide and free magnesium oxide in the steel slag after treatment.
[0039] Application Examples
[0040] Take the steel slag treated in Example 1 or Example 3, mix it with different types of cement according to the mass ratio listed in Table 3 to prepare cement-based material specimens, and conduct stability tests. The stability test of the specimens is carried out in accordance with the national standard GB / T 750-1992 "Cement Autoclave Stability Test Method", and the linear expansion rate of the specimens is measured. The mixing scheme and test results are shown in Table 3:
[0041] Table 3.
[0042]
[0043]
[0044] As can be seen from Table 3, when the steel slag obtained by the harmless treatment method of the present invention is mixed with silicate cement or sulphoaluminate cement to prepare cement-based building materials, the amount of harmless steel slag mixed in each part of cement is in the range of 0.1-2 parts, and the obtained cement-based materials can have good stability; especially the harmless steel slag obtained by the method of Example 3, when used in the preparation of cement-based materials, shows a relatively lower linear expansion rate. However, when the amount of harmless steel slag mixed in each part of cement reaches 2.5 parts (Comparative Example 1), expansion cracking occurs during the experiment, indicating that when the harmless steel slag of the present invention is mixed with cement to prepare cement-based materials, the addition ratio should not be higher than 2:1.
Claims
1. A method for harmless treatment of steel slag, comprising grinding the steel slag with aluminum sulfate material and / or alum material to a specific surface area of not less than 200m 2 / kg.
2. The method according to claim 1, characterized in that: The sum of the masses of the aluminum sulfate materials and the alum materials accounts for no less than 1% of the mass of the steel slag; in a preferred embodiment, the sum of the masses of the aluminum sulfate materials and the alum materials accounts for 2% to 20% of the mass of the steel slag; more preferably 4% to 15%; further preferably 4% to 10%; and most preferably 7% to 10%.
3. The method according to claim 1, characterized in that: The aluminum sulfate material is a combination of one or more of industrial aluminum sulfate, aluminum sulfate 18hydrate, aluminum sulfate hexadecahydrate, and anhydrous aluminum sulfate; the preferred aluminum sulfate material is aluminum sulfate hexadecahydrate or aluminum sulfate 18hydrate; aluminum sulfate 18hydrate is most preferred.
4. The method according to claim 1, characterized in that: The alum material is a combination of one or more of potassium aluminum sulfate dodecahydrate, sodium aluminum sulfate dodecahydrate, and amine aluminum sulfate dodecahydrate; the preferred alum material is sodium aluminum sulfate dodecahydrate or potassium aluminum sulfate dodecahydrate; and potassium aluminum sulfate dodecahydrate is most preferred.
5. The method according to claim 1, characterized in that: A grinding aid is added during the grinding process; the grinding aid can be selected from any one of triethanolamine, ethylene glycol, propylene glycol, sodium sulfate, gypsum, fatty acids and their salts, phosphates, glycerol or polycarboxylates, or a combination of at least two thereof.
6. The method according to claim 1, characterized in that: The joint grinding is grinding to a specific surface area of 200m 2 / kg~1000m 2 / kg; preferably 400m 2 / kg~800m 2 / kg; 400m3 is the most preferred 2 / kg.
7. A steel slag harmless to building materials, obtained by the harmless treatment method according to any one of claims 1 to 6; the free calcium oxide content in the steel slag harmless to building materials is not higher than 3%, and the free magnesium oxide content is not higher than 1.5%.
8. The use of the steel slag harmless to building materials as claimed in claim 7 in the preparation of building materials, comprising mixing the steel slag harmless to building materials with cement to produce cement-based materials.
9. The use according to claim 8, characterized in that: The mass ratio of the steel slag harmless to building materials to cement is not higher than 2:1; preferably 0.1-1.5:1; more preferably 0.5-1.5:1; further preferably 0.5-1.0:1; most preferably 0.5:
1.
10. The use according to any one of claims 8 to 9, characterized in that: The cement is one of silicate cement and sulphoaluminate cement.
Citation Information
Patent Citations
Liquid grinding aid for preparing steel slag micropowder
CN108424011A
Steel slag activation technology
CN111672582A
Grouting material containing steel slag solid waste-based cementing material
CN115073116A
Efficient and energy-saving superfine steel slag powder preparation method
CN115180849A
Ultralow-carbon magnesium oxide slag cement as well as preparation method and application thereof
CN117003501A