Steel slag tuff Portland cement and preparation method thereof

By adding tuff to steel slag and slag cement, and taking advantage of its grinding aid and water retention properties, the problems of high power consumption and poor performance in the production of steel slag and slag cement have been solved, cement production with low power consumption and excellent performance has been achieved, and concrete has been improved. strength and impermeability.

CN118754469APending Publication Date: 2024-10-11赵廷刚
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411001719.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing production of steel slag slag Portland cement has problems such as high power consumption, high equipment costs, poor product performance, poor water retention and bleeding on the concrete surface, resulting in its rare use in practical applications.

Method used

In the cement preparation process of steel slag, slag and gypsum, a certain proportion of tuff is added, and its properties of grinding aid and good water retention are used to reduce power consumption and improve the sphericity and water retention of cement through the combined grinding process of roller press and ball mill. sex.

Benefits of technology

It achieves cement production with low power consumption and excellent performance, improves the strength and impermeability of concrete, reduces bleeding on the concrete surface, and improves the overall performance of the concrete structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004961756030000071
    Figure BDA0004961756030000071
Patent Text Reader

Abstract

The invention belongs to the field of building materials, and discloses steel slag tuff Portland cement and a preparation method thereof. The steel slag tuff Portland cement comprises the following components in percentage by mass: 5-70% of steel slag, 0-34% of mineral slag, 5-40% of tuff, 0-80% of Portland cement clinker and 0-15% of gypsum, and the total percentage of the raw materials is 100%. The tuff is used for assisting grinding, so that the energy consumption is low. The steel slag tuff Portland cement has the advantages of good water-retaining property and good cohesiveness, can well wrap gravel aggregate, does not cause or reduce gravel segregation, improves the uniformity of concrete, and is not only suitable for concrete engineering, but also suitable for construction, tile pasting, wall plastering and other decoration engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of building materials, and particularly relates to steel slag tuff silicate cement and a preparation method thereof. Background Art

[0002] Steel slag is an industrial solid waste produced in the steelmaking process. The current recycling is mainly to return the high-iron content to the steelmaking process after crushing and magnetic separation to replace part of the slag-making materials and scrap steel, while the low-magnetic and low-iron content are mainly used as paving stones and have very low value. Although the country has the GB / T13590-2022 "Steel Slag and Mineral Slag Portland Cement" standard, it is difficult to grind steel slag and mineral slag into fine powder due to their poor grindability. The power consumption of the ball mill system is too high, and the vertical mill system is used for production. The equipment used is expensive, resulting in large investment and poor product performance. The fine powder produced is mostly needle-shaped, with low sphericity and poor fluidity. In addition, the water retention of steel slag and mineral slag silicate cement is poor, and the surface of the concrete is seriously bleeding, affecting the structure and strength of the concrete. Therefore, the production of steel slag and mineral slag cement is very small, and steel slag and mineral slag silicate cement is rarely used in actual applications.

[0003] Steel slag contains tricalcium silicate, dicalcium silicate and iron phase solid solution, which are similar to the hydraulic cementitious materials of Portland cement clinker. After adding appropriate amount of gypsum and grinding into powder, it becomes hydraulic cementitious material, commonly known as cement. Steel slag itself is a low-grade Portland cement clinker. Summary of the invention

[0004] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the primary purpose of the present invention is to provide a steel slag tuff silicate cement.

[0005] The present invention utilizes the silicate cement clinker characteristics of steel slag to produce a cement with low power consumption, excellent performance and simple production method, so that steel slag can be used in a green way while improving the economic value of steel slag. Through a large number of experiments, in the process of preparing cement, a certain proportion of volcanic ash material tuff is added in the process of preparing cement with silicate cement clinker, steel slag, slag and gypsum as component materials, which not only plays a good grinding aid role, but also greatly shortens the grinding time, greatly reduces the grinding power consumption, and also improves the cement performance. Due to the volcanic ash characteristics of tuff, the water retention of cement is improved, the water exudation on the concrete surface is reduced or even eliminated, the concrete structure is improved, and the concrete strength, impermeability, acid and alkali corrosion resistance, etc. are improved.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned steel slag tuff silicate cement.

[0007] The present invention can be easily realized by the existing cement plant roller press ball mill combined with cement grinding system, and is simple to promote. It can also be realized by a separate ball mill system. However, a separate ball mill system basically cannot meet the national energy consumption indicators, and the power consumption exceeds the standard, so it is not recommended.

[0008] The purpose of the present invention is achieved through the following solutions:

[0009] The invention discloses a steel slag tuff silicate cement, which comprises, by weight percentage, 5-70% of steel slag, 0-34% of slag, 5-40% of tuff, 0-80% of silicate cement clinker and 0-15% of gypsum, and the above raw materials total 100%.

[0010] The amount of gypsum added is such that the mass percentage of sulfur trioxide in the slag tuff silicate cement is ≤4.0%.

[0011] The slag tuff silicate cement may also include one or more of limestone, volcanic ash material, fly ash and sandstone in a mass percentage not greater than 20% that meets the quality requirements of cement admixtures.

[0012] The steel slag tuff silicate cement may also include a grinding aid in an amount not greater than 1% by mass; the grinding aid meets the requirements of GB / T26748 "Cement Grinding Aids".

[0013] The preparation method of the steel slag tuff silicate cement comprises the following steps: weighing various raw materials according to the formula, adding them into a roller press, rolling, selecting powder, and ball milling to obtain the steel slag tuff silicate cement.

[0014] The preparation method of the steel slag tuff silicate cement specifically comprises the following steps:

[0015] Each raw material is measured according to the set ratio by the metering equipment, and then fed into the roller press through the conveying equipment. After being rolled by the roller press, it enters the powder selection equipment. Those that meet the fineness requirements enter the ball mill for further grinding, and those that do not meet the fineness requirements return to the roller press for further rolling. The material ground by the ball mill can be directly used as the finished cement product. This production method is called open circuit production. The material after ball milling is sent to the powder selection machine through the conveying equipment. The material with qualified fineness is used as the finished product and enters the cement storage. The material with unqualified fineness returns to the ball mill for further grinding. This method is called closed circuit production. There are also some that select the material with qualified fineness from the material after rolling by the roller press, mix it with the finished product after ball milling and directly add it to the finished product.

[0016] The mechanism of the present invention is:

[0017] The present invention utilizes the characteristic that tuff has a good grinding aid effect on steel slag and ore slag. The production method adopts the roller press and ball mill combined grinding process commonly used in cement plants. Not only is the power consumption low, but also the high sphericity of the product is guaranteed, so that the cement obtained by the present invention has higher strength and better construction performance.

[0018] Tuff is a hard volcanic ash material with good water retention and cohesiveness. Therefore, the addition of tuff in the present invention not only reduces the power consumption of production, but also improves the water retention and cohesiveness of cement, improves or even eliminates the bleeding phenomenon on the surface of concrete, and makes the surface structure of concrete good and the strength high.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0020] (1) The steel slag tuff silicate cement obtained by the present invention has good water retention and cohesiveness, can wrap sand and stone aggregates well, does not cause or reduces sand and stone segregation, and improves the uniformity of concrete. It is not only suitable for concrete engineering, but also suitable for masonry, tile pasting, wall plastering and other decoration projects.

[0021] (2) The present invention can even be produced entirely with solid waste, achieving "zero" silicate cement clinker production of silicate cement. Gypsum can use industrial by-product gypsum, and tuff can use tuff sand washing tailings and tuff gold mine gold extraction tuff tailings, which is low in cost. Tuff is used to assist grinding, which has low energy consumption. DETAILED DESCRIPTION

[0022] The present invention is further described in detail below in conjunction with the examples, but the embodiments of the present invention are not limited thereto. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0023] Unless otherwise specified, the reagents used in the examples can be purchased from the market.

[0024] The percentages of the sieve residues described below are percentages by mass.

[0025] In the preparation of this field, the effect that the experimental small mill can achieve is more perfect for the roller press ball mill combined with cement grinding system used in production, which can also achieve the effect that the 45μm sieve residue of cement products is less than 30%. The original national standard GB175-2007 "General Portland Cement" requires that the cement fineness 45μm sieve residue ≤30%. The new national standard GB175-2023 "General Portland Cement" no longer has this requirement, and is changed to cement fineness 45μm sieve residue ≥5%.

[0026] Example 1

[0027] Calculated by mass percentage, it includes 65% steel slag, 20% tuff, 10% slag, and 5% gypsum, with a total amount of 5000 grams.

[0028] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 60 minutes to obtain steel slag tuff silicate cement.

[0029] The obtained steel slag tuff silicate cement was tested with a 45 μm standard sieve, and the sieve residue was 8.1%.

[0030] The compressive strength of cement mortar was tested in accordance with the national standard GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)", and the 7-day compressive strength was 7.5MPa and the 28-day compressive strength was 14.2MPa, meeting the strength requirements of masonry cement M12.5 (the national standard requires 7-day compressive strength ≥7.0MPa and 28-day compressive strength ≥12.5MPa).

[0031] Example 2

[0032] Calculated by mass percentage, it includes 20% silicate cement clinker, 45% steel slag, 20% tuff, 10% slag, and 5% gypsum, with a total amount of 5000 grams.

[0033] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 50 minutes to obtain steel slag tuff silicate cement.

[0034] The obtained steel slag tuff silicate cement was tested with a 45 μm cement testing standard sieve, and the sieve residue was 8.4%.

[0035] The compressive strength of cement mortar was tested in accordance with the national standard GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)", and the 7-day compressive strength was 12.7MPa and the 28-day compressive strength was 25.8MPa, meeting the strength requirements of masonry cement M22.5 (the national standard requires 7-day compressive strength ≥10.0MPa and 28-day compressive strength ≥22.5MPa).

[0036] Example 3

[0037] Calculated by mass percentage, it includes 35% silicate cement clinker, 30% steel slag, 20% tuff, 10% slag, and 5% gypsum, with a total amount of 5000 grams.

[0038] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 45 minutes to obtain steel slag tuff silicate cement.

[0039] The obtained steel slag tuff silicate cement was tested with a 45 μm cement testing standard sieve, and the sieve residue was 7.4%.

[0040] The compressive strength was tested according to the national standard GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)". The 3-day compressive strength was 15.7MPa and the 28-day compressive strength was 35.8MPa, meeting the strength requirements of masonry cement M32.5 (the national standard requires a 3-day compressive strength of ≥10.0MPa and a 28-day compressive strength of ≥32.5MPa).

[0041] Example 4

[0042] Calculated by mass percentage, it includes 50% silicate cement clinker, 20% steel slag, 15% tuff, 10% slag, and 5% gypsum, with a total amount of 5000 grams.

[0043] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 40 minutes to obtain steel slag tuff silicate cement.

[0044] The obtained steel slag tuff silicate cement was tested with a 45 μm cement testing standard sieve, and the sieve residue was 7.6%.

[0045] According to the national standard GB / T 17671-2021 "Test Method for Cement Mortar Strength (ISO Method)", the compressive strength was tested and the 3-day compressive strength was 22.6MPa and the 28-day compressive strength was 46.2MPa, reaching the strength of 42.5 grade of general Portland cement. (The national standard requires the 3-day compressive strength to be ≥17.0MPa and the 28-day compressive strength to be ≥42.5MPa)

[0046] Example 5

[0047] Calculated by mass percentage, it includes 70% silicate cement clinker, 10% steel slag, 5% tuff, 10% slag, and 5% gypsum, with a total amount of 5000 grams.

[0048] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 35 minutes to obtain steel slag tuff silicate cement.

[0049] The obtained steel slag tuff silicate cement was tested with a 45 μm cement testing standard sieve, and the sieve residue was 7.6%.

[0050] The compressive strength of cement mortar was tested in accordance with the national standard GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)", and the 3-day compressive strength was 30.7MPa and the 28-day compressive strength was 55.8MPa, meeting the strength requirements of general Portland cement grade 52.5 (the national standard requires a 3-day compressive strength of ≥22.0MPa and a 28-day compressive strength of ≥52.5MPa).

[0051] Test Example 1: Water Retention Test

[0052] (1) Calculated by mass percentage, it includes 35% silicate cement clinker, 30% steel slag, 30% slag, and 5% gypsum, with a total amount of 5000 grams.

[0053] The above raw materials were mixed and ground with a small mill in the cement plant laboratory for 180 minutes to obtain steel slag slag silicate cement.

[0054] The obtained steel slag slag silicate cement was tested with a 45 μm standard sieve, and the sieve residue was 16.2%.

[0055] According to the GB / T3183-2017 "Masonry Cement" standard, the water retention rate was tested and the measured water retention rate was 70.6%.

[0056] (2) 4000 g of the slag slag silicate cement prepared by the above method was added with 1000 g of tuff powder with a 45 μm standard sieve residue of 5.3%, and the mixture was thoroughly mixed to prepare a slag tuff silicate cement sample. Using the same method, the water retention rate was measured to be 85.8%.

[0057] The above data prove that the water retention rate of cement is greatly improved after adding tuff powder.

[0058] Test Example 2: Test on the Grinding Performance of Tuff on Steel Slag and Mineral Slag

[0059] The steel slag, slag and tuff were dried and then ground using a 500×500mm small test mill specially used in the laboratory of a cement plant. Each time, 5 kg of material was used. Five grinding time tests were conducted: 30 minutes, 60 minutes, 90 minutes, 120 minutes and 150 minutes.

[0060] The powders obtained by grinding steel slag for 30 minutes, 60 minutes, 90 minutes, 120 minutes and 150 minutes were tested with a 45μm cement test standard sieve, and the sieve residues were 42.3%, 30.7%, 23.4%, 19.7% and 19.6% respectively.

[0061] The powders obtained by grinding slag for 30 minutes, 60 minutes, 90 minutes, 120 minutes and 150 minutes were tested with a 45μm cement test standard sieve, and the sieve residues were 33.3%, 25.7%, 18.4%, 13.7% and 13.6% respectively.

[0062] The powders obtained by grinding tuff for 30 minutes, 60 minutes, 90 minutes, 120 minutes and 150 minutes were tested with a 45μm cement test standard sieve, and the sieve residues were 5.3%, 0%, 0%, 0% and 0% respectively.

[0063] According to the above data, steel slag and ore slag are difficult to grind, especially on the small mill used in the cement plant laboratory. After 120 minutes, the grinding efficiency is basically gone. Tuff is easy to grind, and the 45μm sieve residue is zero after 60 minutes.

[0064] Experimental study on the grinding performance of tuff on steel slag and ore slag

[0065] 3000g of steel slag + 2000g of tuff were put into a special small mill for cement plant and ground for 30 minutes, 60 minutes and 90 minutes respectively. The obtained powder was tested with 45μm cement test standard sieve, and the residues on the sieve were 14.3%, 5.2% and 2.1% respectively.

[0066] 3000g slag + 2000g tuff were put into a small mill specially used in cement plants and ground for 30 minutes, 60 minutes and 90 minutes respectively. The obtained powders were tested with a 45μm cement test sieve, and the residues on the sieve were 12.3%, 5.0% and 1.9% respectively.

[0067] According to the experimental data, it can be clearly seen that tuff has a good grinding aid effect on steel slag and mineral slag. Using tuff to aid grinding of steel slag and mineral slag can greatly reduce power consumption.

[0068] Test Example 3: Compressive Strength Test

[0069] 5 kg of tuff was ground with a small experimental mill for 40 minutes to obtain tuff powder with a 45 μm sieve residue and 0.3%.

[0070] Mineral powder and tuff powder mixture: by mass percentage, including 85% mineral powder and 15% tuff powder mixture.

[0071] Sample 1: 96% Portland cement clinker and 4% gypsum by mass percentage. The sample was prepared by a small grinder in the laboratory of a cement plant with a cement fineness of 9.8% on a 45 μm sieve.

[0072] Sample 2: by mass percentage, including 50% sample 1 and 50% mineral powder.

[0073] Sample 3: by mass percentage, it includes 50% sample 1 and 50% mineral powder and tuff powder mixture.

[0074] According to the national standard GB / T 17671-2021 "Test method for strength of cement mortar (ISO method)", the compressive strength tests were carried out on sample 1, sample 2, and sample 3 respectively, and the results are shown in Table 1.

[0075] Table 1 Compressive strength of cement 1-3

[0076]

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A steel slag tuff silicate cement, characterized in that: Calculated by mass percentage, it includes 5-70% steel slag, 0-34% slag, 5-40% tuff, 0-80% silicate cement clinker, and 0-15% gypsum, and the above raw materials total 100%.

2. The steel slag tuff silicate cement according to claim 1, characterized in that: The amount of gypsum added is such that the mass percentage of sulfur trioxide in the slag tuff silicate cement is ≤4.0%.

3. The steel slag tuff silicate cement according to claim 1, characterized in that: The steel slag tuff silicate cement also includes materials meeting the quality requirements of cement admixtures in a weight percentage not greater than 20%.

4. The steel slag tuff silicate cement according to claim 3, characterized in that: The materials meeting the quality requirements of cement admixtures include one or more of limestone, volcanic ash materials, fly ash, and sandstone.

5. The steel slag tuff silicate cement according to claim 1, characterized in that: The steel slag tuff silicate cement also includes a grinding aid in an amount not greater than 1% by weight.

6. The method for preparing the slag tuff silicate cement according to any one of claims 1 to 5, characterized in that: The following steps are involved: The raw materials are weighed according to the formula, put into a roller press, rolled, powdered, and ball-milled to obtain steel slag tuff silicate cement.

Citation Information

Patent Citations

  • Activation of natural pozzolan and use thereof

    CN113490651A