Belite cement clinker, preparation method thereof and Belite Portland cement

By designing multi-scale defects and chemical doping technology in Belite cement clinker, its strength and durability at each age are improved, solving the problem of low early strength of traditional Portland cement clinker and achieving high efficiency, energy saving and reduction. emissions and resource utilization.

CN118754471AActive Publication Date: 2024-10-11BEIJING BUILDING MATERIALS ACADEMY OF SCI RES

Patent Information

Application Number
CN202410873028.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-01
Publication Date
2024-10-11
Estimated Expiration
2044-07-01

AI Technical Summary

Technical Problem

The existing traditional Portland cement clinker with Belite as the main mineral has low early strength and 28-day strength, cannot meet the requirements of modern concrete construction cycle, and has limited life cycle energy saving and emission reduction effects.

Method used

Belite cement clinker is used, its mineral composition includes C3S 5%~65%, C2S 20%~80%, C3A 1%~8%, C4AF 5%~15%, C5S2Ṡ1~3%, C10S4ṠF21~3%, by designing multi-scale defects in dicalcium silicate crystals, combined with chemical doping technology of low-grade limestone, gypsum and fluorite, to improve hydration activity and crystallization Stress, significantly improve the strength of each age and reduce the heat of hydration.

Benefits of technology

It significantly improves the early and late strength of Belite cement, meets the requirements of modern concrete construction cycle, reduces the heat of hydration and CO2 emissions, improves durability, and achieves efficient resource utilization and production cost reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754471A_ABST
    Figure CN118754471A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, in particular to belite cement clinker, a preparation method of the belite cement clinker and belite Portland cement, and the belite cement clinker comprises the following mineral components: 5%-60% of C3S, 25%-80% of C2S, 1%-8% of C3A, 5%-15% of C4AF, 1%-3% of C5S, 1%-3% of C10S4F and less than 1.0% of free calcium oxide, and the free calcium oxide represents sulfur trioxide. The Belite cement clinker disclosed by the invention is prepared into a proper amount of gypsum to produce a cement product, the 3d strength of the cement product is 13-35MPa, the 28d strength of the cement product can reach 60-70MPa, and the 56d strength of the cement product can reach 72MPa.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a Belite cement clinker and a preparation method thereof, and Belite Portland cement. Background Art

[0002] High-belite cement is a cement with dicalcium silicate (C2S) as the main mineral. It has incomparable advantages over general-purpose Portland cement, such as low firing temperature, low hydration heat release, high later strength, and low CO2 emissions. It has been widely recognized. However, the existing traditional Portland cement clinker with belite as the main mineral has the problem of very low early strength and 28d strength, which cannot meet the requirements of modern concrete construction cycle, and the energy-saving and emission-reduction effects during its life cycle are also very limited. Summary of the invention

[0003] In order to solve the above technical problems of the present invention, the present invention provides a Belite cement clinker and a preparation method thereof and Belite Portland cement.

[0004] According to a first aspect of the present invention, the present invention provides a belite cement clinker, wherein the mineral composition of the belite cement clinker comprises, by weight percentage: C3S 5%-65%, C2S 20%-80%, C3A 1%-8%, C4AF 5%-15%, C5S2Ṡ1-3%, C 10 S4ṠF21~3%, free calcium oxide is less than 1.0%, where Ṡ represents sulfur trioxide.

[0005] In the above scheme, the mineral composition of the Belite cement clinker of the present invention includes calcium sulfosilicate (C5S2Ṡ), calcium fluorosulfosilicate (C5S2Ṡ), and calcium fluoride. 10 These mineral components produce crystallization stress in the cooling process, and realize the multi-scale defect design targets such as points, lines, surfaces, volumes and microcracks in the dicalcium silicate crystal particles, which significantly improves the strength of high-belite cement at all ages, greatly reduces the hydration heat, and improves durability, so that silicate cement with belite as the main mineral can meet the requirements of modern concrete construction cycle.

[0006] Furthermore, the mineral composition of the Belite cement clinker includes, by weight percentage: C3S 10%-50%, C2S 25%-70%, C3A 3%-7%, C4AF 9%-13%, C5S2Ṡ1-3%, C 10 S4ṠF21~2.5%, free calcium oxide less than or equal to 0.30%.

[0007] Furthermore, the Belite cement clinker is calcined from cement raw meal, and the cement raw meal includes, by weight percentage, siliceous aluminum materials, limestone, iron correction materials, gypsum and fluorite; wherein the mass content of calcium oxide in the limestone is greater than or equal to 40%; preferably, the cement raw meal includes the following components in weight percentage: siliceous aluminum materials are 14% to 32%, limestone is 67% to 85%, iron correction materials are 0 to 5.0%, gypsum (calculated as SO3) is greater than 2.0% and less than or equal to 3.5%, and fluorite (calculated as calcium fluoride) is greater than 0.38% and less than or equal to 1.53%.

[0008] In the above scheme, the cement raw materials used in Belite cement clinker include siliceous and aluminous materials, limestone, iron correction materials, gypsum and fluorite. Low-grade limestone is used as calcium raw material, and gypsum and fluorite are used as dopants. The main component of gypsum is calcium sulfate, and the main component of fluorite is calcium fluoride. Through chemical doping technology, the electron cloud direction of dicalcium silicate crystal is successfully changed, which is beneficial to improve the regional distribution of hydration activity. At the same time, trace elements are doped to form calcium sulfosilicate and calcium fluorsulfosilicate minerals with relatively large unit cell volumes, which generate crystallization stress in the cooling process, and realize multi-scale defect design targets such as points, lines, surfaces, volumes and microcracks in dicalcium silicate crystal particles, significantly improve the strength of Belite cement at all ages, greatly reduce the hydration heat (more than 30%), and improve the durability by 15%~200%, so that silicate cement with Belite as the main mineral meets the requirements of modern concrete construction cycle. Compared with ordinary high-belite cement clinker, the Belite cement clinker of the present invention has very outstanding early strength and late strength. When applied to cement, the 3d strength increases by more than 2 times, the 28d strength increases by more than 20MPa, and the 56d strength is as high as 93MPa. The cement prepared by the Belite cement clinker of the present invention has low hydration heat and excellent cement mortar flow properties. At the same time, the comparison of the production of ordinary cement clinker using the same production line shows that the heat consumption of each ton of Belite cement clinker is reduced by 5~20%. In addition, the existing cement clinker generally uses high-grade limestone with a calcium oxide mass content of more than 48% as raw material during the preparation process, while the preparation method of the present invention only needs to use a calcium oxide mass content of greater than or equal to 40%. Reducing the amount of limestone can reduce CO2 emissions and reduce NO x Emissions can be reduced by more than 50%, and the amount of ammonia used in SNCR can be reduced by more than 30%.

[0009] Furthermore, the gypsum is selected from desulfurized gypsum, phosphogypsum, fluorinated gypsum or natural gypsum.

[0010] In the above scheme, the calcium oxide content in the limestone is further limited to be greater than or equal to 40%, so that low-grade limestone can be further used, which significantly improves resource utilization efficiency and reduces production costs.

[0011] Further, the siliceous and aluminous materials include aluminum-based solid waste, and the aluminum-based solid waste includes one or more of sandstone, high-silicon tailings, coal-based solid waste or red mud; and / or, the iron correction material includes one or more natural materials or bulk solid waste containing iron oxide; preferably, the iron correction material includes one or more of iron ore, iron tailings, steel slag or copper slag.

[0012] In the above scheme, selecting aluminum-based solid waste including sandstone or high-silicon tailings as raw materials can significantly improve the efficiency of resource utilization. The comprehensive blending ratio of high-silicon tailings and siliceous-aluminous solid waste (fly ash, coal gangue, red mud, etc.) can reach more than 30%, which can dispose of a large amount of industrial solid waste and save natural clay resources. At the same time, by using iron correction materials such as iron tailings, steel slag, and red mud, with a blending amount of up to 15%, the calcium oxide content of low-grade limestone with high silicon and high aluminum content can be reduced to below 40%.

[0013] According to a second aspect of the present invention, the present invention also provides a method for preparing the above-mentioned Belite cement clinker, comprising the following steps: Step (1): mixing the silicon-alumina material, limestone, iron correction material, gypsum and fluorite in proportion and grinding them to form cement raw material; Step (2): pre-decomposing the cement raw material; Step (3): calcining the pre-decomposed material and then cooling it to obtain cement clinker.

[0014] In the above scheme, the preparation method of Belite cement clinker of the present invention first mixes siliceous aluminum material, limestone, gypsum and fluorite in proportion and then grinds them to form cement raw material, then puts the formed cement raw material into a decomposition furnace for pre-decomposition, and then puts the pre-decomposed material into a rotary kiln for calcination. After firing, it stays for a period of time and cools to obtain cement clinker, thereby realizing large-scale industrial production using a new dry cement rotary kiln process system.

[0015] Furthermore, in step (1), the particle size after grinding is 0.08 mm and the residue on the square hole sieve is less than 15%.

[0016] In the above scheme, by limiting the particle size of the ground material, it is beneficial to improve the subsequent cement raw material calcination efficiency.

[0017] Furthermore, in step (2), the outlet temperature of the pre-decomposition furnace is controlled at 855°C-875°C.

[0018] In the above scheme, by limiting the outlet temperature of the decomposition furnace within a reasonable range, it is beneficial to maintain the performance of the pre-decomposition product.

[0019] Furthermore, in step (3), the calcination temperature is 1300-1400° C., and the calcination time is 10 min-15 min.

[0020] In the above scheme, the calcination temperature of the present invention is about 100°C lower than that of ordinary Portland cement clinker, which saves heat consumption and reduces CO2 and NO x emissions and increase hourly output by more than 8%.

[0021] According to the third aspect of the present invention, the present invention also provides a Belite Portland cement prepared from the above-mentioned Belite cement clinker.

[0022] Furthermore, the preparation method is specifically adopted as follows: the Belite cement clinker and gypsum are ground, and the particle size after grinding is less than 5% on a 0.08 mm square hole sieve and more than 5% on a 0.045 mm square hole sieve, so as to prepare the Belite Portland cement.

[0023] Furthermore, the 3-day strength of Belite Portland cement is 13MPa~35MPa, the 28-day strength is 60MPa~70MPa, the 56-day strength is greater than or equal to 72MPa, and the specific surface area is 340-360m 2 / kg, 3-day hydration heat ≤270J / g, 7-day hydration heat ≤320J / g.

[0024] The technical solution provided by the present invention has the following beneficial effects: The cement raw materials used in the Belite cement clinker of the present invention include siliceous and aluminum materials, limestone, iron correction materials, gypsum and fluorite. Low-grade limestone is used as a calcium raw material, and first gypsum and fluorite are used as dopants. The main components of gypsum are calcium sulfate, and the main components of fluorite are calcium fluoride. Through chemical doping technology, the electron cloud direction of dicalcium silicate crystals is successfully changed, which is beneficial to improving the regional distribution of hydration activity. At the same time, trace elements are doped to form calcium sulfosilicate and calcium fluorsulfosilicate minerals with larger unit cell volumes than dicalcium silicate, generate crystallization stress in the cooling process, realize multi-scale defect design targets such as points, lines, surfaces, volumes and microcracks in dicalcium silicate crystal particles, and significantly improve the strength of high Belite cement at all ages. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1It is a SEM picture of the Belite cement clinker of Example 4 of the present invention.

[0027] Figure 2 3 is the BSE diagram of the belite cement clinker of Example 4 of the present invention.

[0028] Figure 3 is the O in the Belite cement clinker of Example 4 1s Orbital electron chemical shift X-ray photoelectron spectroscopy analysis results.

[0029] Figure 4 The XPS-Ca in the Belite cement clinker of Example 4 2p Orbital electron chemical shift X-ray photoelectron spectroscopy analysis results. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The beneficial effects of the present invention will be described below in conjunction with specific embodiments and comparative examples.

[0032] Example 1

[0033] Embodiments 1-5 provide a Belite cement clinker, which is calcined from cement raw materials, wherein the cement raw materials include siliceous aluminum materials, limestone, iron correction materials, gypsum and fluorite, wherein the siliceous aluminum materials are 14% to 32%, the limestone is 67% to 85%, the iron correction materials are 0 to 5.0%, the gypsum (in terms of SO3) is greater than 2.0% and less than or equal to 3.5%, and the fluorite (in terms of calcium fluoride) is greater than 0.38% and less than or equal to 1.53%, and their respective mineral compositions are shown in Table 1 below. Among them, the gypsum is selected from desulfurized gypsum, and the content of calcium oxide in the limestone is 45%. The siliceous aluminum materials include aluminum-based solid waste, and the aluminum-based solid waste includes sandstone, high-silicon tailings, coal-based solid waste and red mud, and the iron correction materials include iron ore, iron tailings, steel slag and copper slag.

[0034] The preparation method of Belite cement clinker is as follows: Step (1): Mix the silicon-alumina material, iron correction material, limestone, gypsum and fluorite in appropriate proportions and grind them. The particle size after grinding is required to be less than 15% on a 0.08 mm square hole sieve to form cement raw material.

[0035] Step (2): The cement raw material enters the new dry process cement rotary kiln production process system equipped with a preheating and pre-decomposition system, and is pre-decomposed in the decomposition furnace. The outlet temperature of the decomposition furnace is controlled at 865±10℃.

[0036] Step (3): After pre-decomposition, the material enters the rotary kiln and is calcined at 1350±50°C, passing through the sintering zone for 10min~15min, and then cooled to obtain Belite cement clinker. The mineral composition of the obtained Belite cement clinker is shown in Table 2 below.

[0037] Comparative Example 1

[0038] This comparative example provides a belite cement clinker, which is different from Example 1 in that it does not contain fluorite and gypsum.

[0039] Comparative Example 2

[0040] This comparative example provides a belite cement clinker, which is different from Example 1 in that it contains gypsum but not fluorite.

[0041] Comparative Example 3

[0042] This comparative example provides a belite cement clinker, which is different from Example 1 in that it contains fluorite but does not contain gypsum.

[0043] The mineral composition of the belite cement clinker obtained in Comparative Examples 1-3 is shown in Table 2 below.

[0044] Table 1

[0045] Table 2

[0046] The Belite cement clinker and gypsum of Examples 1-5 and Comparative Examples 1-3 were ground at a weight ratio of 97.5%:2.5%, and the particle size after grinding was required to be less than 5% on a 0.08 mm square hole sieve and greater than 5% on a 0.045 mm square hole sieve, respectively, to prepare Belite Portland cement. The obtained Belite Portland cement was subjected to performance testing according to GB / T17671-1999 standard test, and the test results are shown in Table 3 below.

[0047] Table 3

[0048] It can be seen from the experimental results in Table 3 that the 3d strength of cement prepared by the high-activity Belite cement clinker of the present invention is between 15 and 35 MPa, the 28d strength can reach 60 MPa to 70 MPa, and the 56d strength is as high as 72 MPa. Compared with P.I42.5 silicate cement (3d hydration heat is greater than or equal to 290 J / g, 7d hydration heat is greater than or equal to 350 J / g), the hydration heat of cement prepared by the high-activity Belite cement clinker of the present invention is reduced by 30 to 50%. When the water-cement ratio is 0.5, the expansion of cement mortar can reach 175 mm to 200 mm, and the hydration heat is low, the stability is good, the working performance is excellent, and the various performance indicators of cement fully meet or exceed the requirements of ASTM 150M and EN197-1 standards. The concrete prepared by the high-performance and high-activity Belite cement prepared by the present invention has a higher 28d strength than the concrete prepared by ordinary P.I42.5 Portland cement, which is improved by more than 10%, and has better durability. The chloride ion permeability coefficient and the electric flux test results are reduced by more than 50%, indicating that the high-activity Belite cement clinker of the present invention has the potential to replace ordinary Portland cement clinker on a large scale to produce general Portland cement.

[0049] The Belite cement clinker of Example 4 of the present invention was subjected to SEM and BSE tests, and the results are as follows: Figure 1 and Figure 2 As shown by Figure 1 and Figure 2 It can be seen that the high-activity belite cement clinker of the present invention has a multi-scale crystal defect design. The research and development is based on quantum mechanics, doping theory, defect design theory, high-temperature thermodynamics theory and surface chemistry theory. Through the reconstruction of the electron cloud distribution of belite crystals and the multi-scale crystal defect design method, the hydration activation point of dicalcium silicate minerals is increased, and the grindability of high belite clinker is improved, thereby significantly improving the early and late strength of belite cement clinker. The green low-carbon silicate cement clinker with high-activity belite as the main mineral is produced using the existing new dry cement process system. The cement performance meets the standard requirements of general silicate cement, achieving the goals of doubling material performance, energy saving, carbon reduction and efficiency improvement, and providing strong technical support for cement companies to achieve green and low-carbon transformation.

[0050] like Figure 3 The oxygen atoms 1s (O 1s ) Orbital electron chemical shift X-ray photoelectron spectroscopy analysis results, Figure 4 The graph shows the calcium 2p (Ca) content in the belite cement clinker of Example 4. 2p ) orbital electron chemical shift X-ray photoelectron spectroscopy analysis results, through Figure 3 and Figure 4It can be seen that the outer electrons of oxygen and calcium elements in the dicalcium silicate mineral crystals have undergone obvious chemical shifts, indicating that the electron cloud distribution of the dicalcium silicate crystal has been reconstructed.

[0051] The results of industrial production tests and engineering application technology research show that various types of cement products prepared using the Belite cement clinker of the present invention not only meet the current general Portland cement product standard requirements, but also can develop high value-added, multifunctional, and multi-purpose special engineering cement products on this basis, such as high (medium) sulfate-resistant cement, offshore Portland cement, nuclear power cement, dam cement, oil well cement, etc. Highly active Belite cement can be used to prepare fiber-reinforced ultra-high performance concrete (FRUHPC) and ultra-durable concrete (UHDC) with a strength grade of up to 250MPa. It has significant performance, quality, cost and environmental advantages over ordinary Portland cement, and will become the basic material for building sustainable green low-carbon infrastructure.

[0052] Compared with ordinary Portland cement clinker, in addition to excellent ultra-high gelling properties, the Belite cement clinker of the present invention has typical characteristics of low energy load, low resource load and low environmental load. After the industrialization of the research and development results, based on the annual replacement of 100 million tons of ordinary Portland cement clinker and the heat consumption of 110 kg of standard coal per ton of ordinary Portland cement clinker, the production of high-activity Belite cement clinker can save about 10% of heat consumption, equivalent to about 1.1 million tons of standard coal, and save 1.65 billion yuan in costs; CO2 emissions can be reduced by up to 5 million tons, saving about 2 billion yuan in costs; the amount of ammonia water can be reduced by 150,000 tons, saving 120 million yuan in costs; 10 million tons of steel slag, 12 million tons of desulfurized gypsum, and 110 million tons of low-grade limestone (CaO content below 45%) can be disposed of, reducing costs by more than 3.5 billion yuan, which not only significantly improves the efficiency of resource use, but also realizes the strategic storage of high-grade original ecological natural resources. In addition, realizing the green and low-carbon transformation of traditional cement enterprises based on existing production lines not only preserves the value of state-owned assets, but also stabilizes the employment rate and maintains social stability.

[0053] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A Belite cement clinker, characterized in that: The mineral composition of the Belite cement clinker includes, by weight percentage: C3S 5%-60%, C2S 25%-80%, C3A 1%-8%, C4AF 5%-15%, C5S2Ṡ1-3%, C 10 S4ṠF21~3%, free calcium oxide is less than 1.0%, where Ṡ represents sulfur trioxide.

2. The Belite cement clinker according to claim 1, characterized in that: The mineral composition of the Belite cement clinker includes, by weight percentage: C3S 10%-50%, C2S 25%-70%, C3A 3%-7%, C4AF 9%-13%, C5S2Ṡ1-3%, C 10 S4ṠF21~2.5%, free calcium oxide less than or equal to 0.30%.

3. The Belite cement clinker according to claim 1, characterized in that: The Belite cement clinker is obtained by calcining cement raw materials, wherein the cement raw materials include siliceous and aluminous materials, limestone, iron correction materials, gypsum and fluorite; wherein the mass content of calcium oxide in the limestone is greater than or equal to 40%.

4. The Belite cement clinker according to claim 3, characterized in that: The gypsum is selected from desulfurized gypsum, phosphogypsum, fluorinated gypsum or natural gypsum.

5. The Belite cement clinker according to claim 3 or 4, characterized in that: The silicon-aluminum material includes aluminum-based solid waste, and the aluminum-based solid waste includes one or more of sandstone, high-silicon tailings, coal-based solid waste or red mud; And / or, the iron correction material includes one or more natural materials or bulk solid wastes containing iron oxide; preferably, the iron correction material includes one or more of iron ore, iron tailings, steel slag or copper slag.

6. The method for preparing Belite cement clinker according to any one of claims 1 to 5, characterized in that: The steps include: Step (1): mixing the silicon-alumina material, limestone, iron correction material, gypsum and fluorite in proportion and grinding them to form cement raw material; Step (2): pre-decomposing the cement raw material; Step (3): calcining the pre-decomposed material and then cooling it to obtain cement clinker.

7. The method for preparing Belite cement clinker according to claim 6, characterized in that: In step (1), the particle size after grinding is required to have a 0.08 mm square hole sieve residue of less than 15%; and / or, in step (2), the outlet temperature of the pre-decomposition furnace is controlled at 855° C. to 875° C.

8. The method for preparing Belite cement clinker according to claim 6, characterized in that: In step (3), the calcination temperature is 1300° C. to 1400° C., and the calcination time is 10 min to 15 min.

9. A Belite Portland cement, characterized in that: Prepared from the Belite cement clinker described in any one of claims 1 to 5.

10. The Belite Portland cement according to claim 9, characterized in that: The 3-day strength of Belite Portland cement is 13MPa~35MPa, the 28-day strength is 60MPa~70MPa, the 56-day strength is greater than or equal to 72MPa, and the specific surface area is 340-360m 2 / kg, 3-day hydration heat ≤270J / g, 7-day hydration heat ≤320J / g.

Citation Information

Patent Citations

  • Belite cement and preparation method thereof

    CN104788032A

  • Method for preparing calcium sulphosilicate-Belite-sulfoaluminate cement clinker at low temperature

    CN110078394A

  • Dicalcium silicate-calcium sulphoaluminate-calcium sulphosilicate cement clinker and preparation process thereof

    CN115849740A

  • Cement composition

    JP2014185040A

Cited By

  • Low-carbon high-belite / high-iron phase mineral material as well as preparation method and application thereof

    CN119430716A

  • Cement clinker for high-speed rail and preparation method thereof

    CN120058250A

  • Cement clinker for high-speed rail and preparation method thereof

    CN120058250B