Underwater rapid anti-seepage and long-acting reinforcing plugging material and preparation method thereof

Through the combination of polyelectrolyte binder, controlled particle size gravel and Portland cement, and the use of underwater chemical bonding and mechanical sealing technology, the stability and strength of the leakage parts of earth-rock dams in the underwater environment are solved. Solve the problem of deficiencies, achieve rapid and efficient sealing and long-term reinforcement, and meet the safety needs of underwater projects.

CN118754544AActive Publication Date: 2024-10-11XIAN UNIV OF TECH

Patent Information

Application Number
CN202410801795.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-11
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

The existing sealing materials for leakage parts of earth-rock dams have problems such as poor stability, insufficient strength, and uncontrollable solidification time in underwater environments, making it difficult to achieve rapid and efficient underwater reinforcement.

Method used

Polycationic electrolytes and polyanionic electrolytes are used to prepare polyelectrolyte binder powder, which is combined with sand and Portland cement with controllable particle sizes, and mixed by ball milling to prepare blocking materials. Underwater chemical bonding and mechanical blocking are used. It imitates the sandcastle worm structure, regulates the setting time and mechanical properties, and forms a mortise-and-tenon structure and chemical bonds to achieve rapid sealing and long-term reinforcement.

Benefits of technology

It achieves rapid and efficient sealing and long-term reinforcement of underwater leakage parts, improves the mechanical properties and stability of sealing materials, meets the safety needs of underwater projects, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an underwater rapid seepage-proofing and long-acting reinforcing plugging material, and also discloses a preparation method of the plugging material, and the preparation method comprises the following steps: step 1, preparing polyelectrolyte adhesive powder by using a polycation electrolyte and a polyanion electrolyte; 2, grit with the particle size being 0.2-2 mm is prepared; 3, Portland cement with the particle size ranging from 0.002 mm to 0.05 mm is prepared; and 4, preparing the plugging material by using the polyelectrolyte adhesive powder prepared in the step 1, grit and Portland cement. The plugging material provided by the invention can realize rapid plugging and long-acting reinforcement of the leakage part of the underwater earth and rockfill dam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of anti-seepage reinforcement plugging materials, and in particular relates to an underwater rapid anti-seepage and long-term reinforcement plugging material. The present invention also relates to a preparation method of the above-mentioned plugging material. Background Art

[0002] Earth-rock dams have natural advantages such as local materials, simple structure, simple construction and easy maintenance, and are widely used in dam construction around the world. There are a large number of earth-rock dams in my country, and most of them were built in the 1950s and 1970s. Therefore, there are problems such as low construction standards, poor construction quality, and aging functions, which pose safety hazards. In addition, under the influence of global climate change, a small number of reservoirs have been in danger, which not only caused loss of life and property, but also brought challenges to the safe operation and management of earth-rock dams. "Targeted" blocking of leakage channels is the key to treating leakage hazards of earth-rock dams. Therefore, how to achieve efficient and rapid blocking and long-term reinforcement of leakage parts of earth-rock dams underwater at the same time has become an urgent problem to be solved.

[0003] At present, plugging materials can be divided into two categories: granular plugging materials and chemical plugging materials. The former is mainly cement materials, while the latter is most representative of polyurethane materials, which are generally configured as slurries that can be poured into leakage channels. Among them, cement plugging materials have the advantages of high stone body strength, good durability, rich material sources, simple process equipment, and low cost, but the stone body formed by it is easy to weather and disintegrate under dry conditions; in the case of long-term water, due to the water solubility of silicates, it is easy to dissolve, the stability is poor, and there is a risk of plugging failure. The polyurethane grouting material is widely used in the reinforcement, anti-seepage and plugging projects of dams and reservoirs with the advantages of low viscosity, good pourability, adjustable gel time from seconds to hours, good impermeability, and no pollution to the environment. However, its strength is low, generally the compressive strength is 6 to 30MPa, and the strength decreases significantly after absorbing water compared to the dry state, which is not conducive to forming a high-strength bond with wet soil and stone, and cannot form a satisfactory reinforcement layer. In addition, the bonding strength of water-soluble polyurethane gel to soil and stone is generally lower than its own tensile strength, resulting in the shrinkage of the gel under dry-wet cycle conditions, causing the bonding interface between the gel and soil and stone to be destroyed and water seepage to occur.

[0004] Therefore, based on the uneven surface of the earth-rock dam and the special underwater environment, developing a new type of sealing material for rapid underwater anti-seepage and long-term reinforcement of the earth-rock dam to achieve long-term underwater reinforcement of the earth-rock dam has become a difficult problem in this field.

[0005] The Chinese patent "A preparation method for reinforcement and water blocking materials for underground coal mines" (application number: CN202310980931.1, publication date: 2023.12.01, publication number: CN117143448A) discloses a preparation method for reinforcement and water blocking materials for underground coal mines. This method adds additives and sulfosalicylic acid to the reinforcement and water blocking materials to prepare a reinforcement and water blocking material with good mechanical properties, antistatic properties and flame retardant properties, which can be effectively used in underground coal mines for reinforcement and water blocking. However, the plugging material prepared by this method has uncontrollable solidification time in a water-rich environment, which is difficult to operate and leads to the risk of failure of emergency repair.

[0006] The Chinese patent "A self-water blocking concrete and its preparation method" (application number: CN202310429493.X, publication date: 2023.09.01, publication number: CN116675483A) discloses a self-water blocking concrete and its preparation method. This method does not add water, and minimizes the water absorption and expansion of the highly absorbent resin SAP during the preparation process, so that the internal material fully maintains the reaction activity, thereby ensuring that the SAP can play its maximum role when the surface material cracks. However, this method only uses the water absorption and expansion effect inside the particles to consolidate and block cracks. It is easy to dehydrate under dry conditions, forming new cracks and causing the matrix to collapse. Summary of the invention

[0007] The purpose of the present invention is to provide an underwater rapid anti-seepage and long-term reinforcement plugging material, which can realize rapid plugging and long-term reinforcement of the leakage part of the underwater earth-rock dam.

[0008] Another object of the present invention is to provide a method for preparing the above-mentioned plugging material.

[0009] The technical solution adopted by the present invention is a method for preparing an underwater rapid anti-seepage and long-term reinforced plugging material, which is specifically implemented according to the following steps:

[0010] Step 1, preparing polyelectrolyte adhesive powder using polycation electrolyte and polyanion electrolyte;

[0011] Step 2, preparing gravel with a particle size of 0.2 to 2 mm;

[0012] Step 3, preparing silicate cement with a particle size of 0.002 to 0.05 mm;

[0013] Step 4: preparing a plugging material using the polyelectrolyte adhesive powder, gravel and silicate cement prepared in the above steps.

[0014] The present invention is also characterized in that:

[0015] In step 1, the polycation electrolyte is one of polyethyleneimine, polyamide-epichlorohydrin or polyvinylpyridine; the polyanion electrolyte is polyacrylic acid or phosphotungstic acid.

[0016] Step 1 is as follows:

[0017] A polycation electrolyte solution with a mass fraction of 5 to 30 wt% is added to a polyanion electrolyte solution with a mass fraction of 5 to 30 wt%, the pH of the mixed solution is adjusted to 5 to 9, magnetic stirring is performed to fully mix the mixed solution, and the mixed solution is immediately immersed in liquid nitrogen for 10 to 60 minutes, freeze-dried to remove excess water, ground and sieved through a 200 to 2000 mesh sieve, and the particle size distribution is controlled to be 0.0002 to 0.075 mm, so as to obtain a polyelectrolyte adhesive powder.

[0018] The volume ratio of the polycation electrolyte solution to the polyanion electrolyte solution is 1-9:9-1.

[0019] The gravel in step 2 is obtained by passing industrial grade gravel through a 8-80 mesh sieve.

[0020] In step 3, industrial-grade silicate cement is sieved and graded using 250-8000 meshes to obtain silicate cement.

[0021] In step 3, the silicate cement is composed of tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium aluminoferrite and gypsum in a mass ratio of 50-70:15-30:5-10:5-10:3-5.

[0022] Step 4 is as follows:

[0023] The polyelectrolyte adhesive powder, gravel and silicate cement in a mass ratio of 1:1-4:2-4 are evenly mixed by ball milling to obtain the plugging material.

[0024] Another technical solution adopted by the present invention is an underwater rapid anti-seepage and long-term reinforced plugging material, which is prepared by the above-mentioned preparation method.

[0025] The beneficial effects of the present invention are:

[0026] The method of the present invention realizes rapid and efficient plugging of leakage parts through underwater chemical bonding imitating sandcastle worms and mechanical plugging with cement, and realizes underwater long-term reinforcement of earth-rock dams by adjusting the size distribution of raw materials, utilizing the mortise and tenon structure between the plugging raw materials and the damaged parts, the capillary action between the raw materials and water, and the chemical bonding between the adhesive and the earth and rock blocks. Firstly, silicate cement, gypsum, sand and gravel with controllable particle size, and polyelectrolyte adhesive powder with controllable particle size that sticks to water when in contact with water are selected as raw materials, and the optimal setting time is controlled by adjusting the ratio of silicate cement and gypsum, and the mechanical properties are controlled by adjusting the ratio of adhesive to cement matrix, so as to meet the optimal operating time and initial strength requirements for emergency repairs in actual underwater working conditions; secondly, the particle size distribution of silicate cement, gypsum, gravel and adhesive powder is adjusted to meet the mortise and tenon structure that matches the earth and rock matrix, so as to improve the bond between the plugging material and the damaged matrix. Mechanical properties; combined with the capillary action of gravel, through mechanisms such as moisture regulation, particle communication, cementation effect and drainage effect, it can effectively improve the stability and strength of the underwater environment of the soil, enhance the water erosion resistance of the soil, and protect the safety and stability of underwater projects and soil structures; at the same time, through the cross-linking effect between the polyelectrolyte adhesive and the soil and rock body, hydrogen bonds, van der Waals forces and other adsorption forces are formed on the surface of the damaged body, thereby achieving long-term reinforcement of the earth-rock dam, and the material of the present invention has low production cost and no special requirements on production equipment, and has good application prospects in the field of anti-seepage reinforcement and plugging materials. DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with specific implementation modes.

[0028] The preparation method of the underwater rapid anti-seepage and long-term reinforcement plugging material of the present invention is specifically implemented according to the following steps:

[0029] Step 1, preparing a polyelectrolyte adhesive powder that becomes sticky when in contact with water;

[0030] The specific steps are as follows: adding a polycation electrolyte solution with a mass fraction of 5 to 30 wt % to a polyanion electrolyte solution with a mass fraction of 5 to 30 wt %, wherein the volume ratio of the polycation electrolyte solution to the polyanion electrolyte solution is 1 to 9:9 to 1, adjusting the pH of the mixed solution to 5 to 9, stirring the mixed solution with magnetic force to fully mix the mixed solution, immediately immersing the mixed solution in liquid nitrogen for 10 to 60 minutes, freeze-drying the mixed solution to remove excess water, and finally grinding the mixed solution with a mortar and passing it through a 200 to 2000 mesh sieve to control the particle size distribution to be 0.0002 to 0.075 mm, thereby obtaining a polyelectrolyte adhesive powder that is sticky when it comes into contact with water.

[0031] The polycation electrolyte is any one of polyethyleneimine (PEI), polyamide-epichlorohydrin (PAE-Cl) or polyvinylpyridine (PVP); the polyanion electrolyte is polyacrylic acid (PAA), phosphotungstic acid (PW 12 )

[0032] Step 2, preparing gravel with controllable capillary particle size;

[0033] The specific steps are: pass industrial-grade gravel through an 8-80 mesh sieve, control its particle size distribution within the range of 0.2-2 mm, and obtain gravel with controllable particle size and capillary action.

[0034] Step 3, preparing silicate cement with controllable particle size;

[0035] The specific steps are: sieving and grading industrial-grade silicate cement with 250-8000 meshes to control the particle size distribution within 0.002-0.05 mm, thereby obtaining silicate cement with controllable particle size;

[0036] Among them, silicate cement is composed of tricalcium silicate (C3S), dicalcium silicate (C2S), tricalcium aluminate (C3A), tetracalcium aluminoferrite (C4AF) and gypsum (CaSO4) in a mass ratio of 50-70:15-30:5-10:5-10:3-5.

[0037] Step 4: Prepare a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0038] The specific steps are: the polyelectrolyte adhesive powder that sticks to water in step 1, the gravel with controllable particle size with capillary action in step 2, and the silicate cement with controllable particle size in step 3 are mixed evenly by ball milling in a mass ratio of 1:1-4:2-4 to obtain a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0039] The method of the present invention can quickly plug leaks and prevent seepage by imitating the underwater bonding of sandcastle worms and the plugging effect of cement, and can realize underwater long-term reinforcement of earth-rock dams by combining mortise and tenon structure, capillary action and chemical bonding. First, silicate cement with controllable solidification time and polyelectrolyte adhesive that sticks to water can form an effective physical barrier, effectively meet the operation time and initial strength required for underwater repair, and achieve the purpose of rapid plugging and leak prevention; secondly, the particle size distribution between the raw materials can be controlled to form a mortise and tenon structure, which can better adapt to the defective earth and stone block matrix and improve the mechanical properties of the plugging material and the matrix; the capillary action of gravel has good moisture regulation, particle communication, cementation effect and drainage effect, so as to enhance the underwater environmental stability and strength of the soil, improve the water erosion resistance, and further improve the underwater stability; finally, the cross-linking effect between the polyelectrolyte adhesive and the soil and stone body forms hydrogen bonds, van der Waals forces and other adsorption forces, which can effectively realize underwater long-term reinforcement of earth-rock dams and improve stability and durability. Therefore, the method of the present invention achieves rapid and efficient underwater plugging and leakage prevention and long-term reinforcement of the earth-rock dam by regulating the material composition, structure and action mechanism, and the three work synergistically.

[0040] Example 1

[0041] Step 1, preparing a polyelectrolyte adhesive powder that becomes sticky when in contact with water;

[0042] A 15 wt% polyamide-epichlorohydrin (PAE-Cl) solution was added to a 10 wt% phosphotungstic acid (PW 12 ) solution, adjusting the volume ratio to 1:9 and pH to 7, and after fully mixing with magnetic stirring, immediately immerse the mixture in liquid nitrogen for 30 minutes and freeze-dry to remove excess water. Finally, grind it with a mortar and pass it through a 500-mesh sieve to control the particle size distribution to about 0.025 mm, and you can get a polyelectrolyte adhesive powder that sticks to water;

[0043] Step 2, preparing gravel with controllable capillary particle size;

[0044] The industrial-grade gravel is passed through a 50-mesh sieve and its particle size distribution is controlled to be about 0.27 mm, so that the gravel with controllable capillary particle size can be obtained;

[0045] Step 3, preparing silicate cement with controllable particle size;

[0046] The tricalcium silicate (C3S), dicalcium silicate (C2S), tricalcium aluminate (C3A), tetracalcium aluminoferrite (C4AF) and gypsum (CaSO4) in industrial-grade silicate cement are sieved and graded with 5000 meshes, and the particle size distribution is controlled to be about 0.0026 mm. The mixture is mixed with gypsum in a mass ratio of 60:25:7:5:3 to obtain silicate cement with controllable particle size.

[0047] Step 4: Prepare a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0048] The polyelectrolyte adhesive powder that becomes sticky when in contact with water in step 1, the gravel with controllable particle size having capillary action in step 2, and the silicate cement with controllable particle size in step 3 are evenly mixed by ball milling in a mass ratio of 25:25:50 to obtain a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0049] Example 2

[0050] Step 1, preparing a polyelectrolyte adhesive powder that becomes sticky when in contact with water;

[0051] A 5 wt% polyamide-epichlorohydrin (PAE-Cl) solution was added to a 30 wt% phosphotungstic acid (PW 12 ) solution, adjusting the volume ratio to 9:1 and the pH to 5, and after fully mixing with magnetic stirring, immediately immerse the mixture in liquid nitrogen for about 10 minutes, and freeze-dry to remove excess water. Finally, grind it with a mortar and pass it through a 1000-mesh sieve, and control the particle size distribution to be around 0.002 mm, and you can get a polyelectrolyte adhesive powder that sticks to water;

[0052] Step 2, preparing gravel with controllable capillary particle size;

[0053] The industrial-grade gravel is passed through an 80-mesh sieve and its particle size distribution is controlled to be about 0.2 mm, so that the gravel with controllable particle size can be obtained with capillary action;

[0054] Step 3, preparing silicate cement with controllable particle size;

[0055] The tricalcium silicate (C3S), dicalcium silicate (C2S), tricalcium aluminate (C3A), tetracalcium aluminoferrite (C4AF) and gypsum (CaSO4) in industrial-grade silicate cement are sieved and graded with 1340 meshes, and the particle size distribution is controlled to be about 0.01 mm. The mixture is composed of gypsum in a mass ratio of 65:20:5:5:5, and silicate cement with controllable particle size can be obtained.

[0056] Step 4: Prepare a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0057] The polyelectrolyte adhesive powder that becomes sticky when in contact with water in step 1, the gravel with controllable particle size having capillary action in step 2, and the silicate cement with controllable particle size in step 3 are evenly mixed by ball milling in a mass ratio of 15:25:60 to obtain a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0058] Example 3

[0059] Step 1, preparing a polyelectrolyte adhesive powder that becomes sticky when in contact with water;

[0060] A 15 wt% polyethyleneimine (PEI) solution was added to a 15 wt% phosphotungstic acid (PW 12 ) solution, adjusting the volume ratio to 6:4 and pH to 7, and after fully mixing with magnetic stirring, immediately immerse the mixture in liquid nitrogen for about 60 minutes, and freeze-dry to remove excess water. Finally, grind it with a mortar and pass it through a 1000-mesh sieve, and control its particle size distribution to about 0.013 mm, and you can get a polyelectrolyte adhesive powder that sticks to water;

[0061] Step 2, preparing gravel with controllable capillary particle size;

[0062] The industrial-grade gravel is passed through a 60-mesh sieve and its particle size distribution is controlled to be about 0.25 mm, so that the gravel with controllable particle size can be obtained with capillary action;

[0063] Step 3, preparing silicate cement with controllable particle size;

[0064] The tricalcium silicate (C3S), dicalcium silicate (C2S), tricalcium aluminate (C3A), tetracalcium aluminoferrite (C4AF) and gypsum (CaSO4) in industrial-grade silicate cement are sieved and graded with 5000 meshes, and the particle size distribution is controlled to be about 0.0026 mm. The mixture is mixed with gypsum in a mass ratio of 60:21:10:5:4 to obtain silicate cement with controllable particle size.

[0065] Step 4: Prepare a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0066] The polyelectrolyte adhesive powder that becomes sticky when in contact with water in step 1, the gravel with controllable particle size having capillary action in step 2, and the silicate cement with controllable particle size in step 3 are evenly mixed by ball milling in a mass ratio of 20:20:60 to obtain a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0067] Example 4

[0068] Step 1, preparing a polyelectrolyte adhesive powder that becomes sticky when in contact with water;

[0069] Add a 15wt% polyethyleneimine (PEI) solution to a 15wt% polyacrylic acid (PAA) solution, adjust the volume ratio to 5:5 and the pH to 8, stir the mixture with magnetic force to mix thoroughly, and then immerse the mixture in liquid nitrogen for about 30 minutes, and freeze-dry to remove excess water. Finally, grind it with a mortar and pass it through a 1000 mesh sieve, and control the particle size distribution to about 0.002mm, and you can get a polyelectrolyte adhesive powder that sticks to water.

[0070] Step 2, preparing gravel with controllable capillary particle size;

[0071] The industrial-grade gravel is passed through an 80-mesh sieve and its particle size distribution is controlled to be about 0.2 mm, so that the gravel with controllable particle size can be obtained with capillary action;

[0072] Step 3, preparing silicate cement with controllable particle size;

[0073] The tricalcium silicate (C3S), dicalcium silicate (C2S), tricalcium aluminate (C3A), tetracalcium aluminoferrite (C4AF) and gypsum (CaSO4) in industrial-grade silicate cement are sieved and graded with 5000 meshes, and the particle size distribution is controlled to be about 0.0026 mm. The mixture is mixed with gypsum in a mass ratio of 65:11:10:10:4 to obtain silicate cement with controllable particle size.

[0074] Step 4: Prepare a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0075] The polyelectrolyte adhesive powder that becomes sticky when in contact with water in step 1, the gravel with controllable particle size having capillary action in step 2, and the silicate cement with controllable particle size in step 3 are evenly mixed by ball milling in a mass ratio of 15:55:30 to obtain a new type of underwater rapid anti-seepage and long-term reinforcement plugging material.

[0076] Table 1 is a comparison table of performance test results of the plugging materials prepared in Examples 1 to 4 of the present invention and the traditional silicate cement plugging materials. The tested performance includes: underwater solidification time after the two materials are compounded with soil and rock blocks, and mechanical properties after underwater immersion for one month.

[0077] Table 1 Performance test results comparison table

[0078]

[0079] It can be seen from the data listed in Table 1 that, compared with the traditional silicate cement plugging material, the new plugging material for underwater rapid anti-seepage and long-term reinforcement of earth-rock dams prepared by the present invention achieves rapid and efficient plugging of underwater leakage parts within 2 minutes due to the synergistic effect of underwater chemical bonding of sandcastle worms and cement mechanical plugging with controllable solidification time; the mortise and tenon structure between the plugging material and the earth and rock blocks, the capillary action between the gravel and water, and the chemical bonding between the adhesive and the earth and rock blocks make the mechanical properties of the composite material of the present invention and the earth and rock blocks still as high as about 150MPa after being immersed in water for one month, and has good mechanical properties, which further improves the underwater stability of the plugging material, thereby achieving long-term reinforcement of the earth and rock dam.

Claims

1. A method for preparing an underwater rapid anti-seepage and long-term reinforcement plugging material, characterized in that: Follow the steps below to implement it: Step 1, preparing polyelectrolyte adhesive powder using polycation electrolyte and polyanion electrolyte; Step 2, preparing gravel with a particle size of 0.2 to 2 mm; Step 3, preparing silicate cement with a particle size of 0.002 to 0.05 mm; Step 4: preparing a plugging material using the polyelectrolyte adhesive powder, gravel and silicate cement prepared in the above steps.

2. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: In step 1, the polycation electrolyte is one of polyethyleneimine, polyamide-epichlorohydrin or polyvinylpyridine; the polyanion electrolyte is polyacrylic acid or phosphotungstic acid.

3. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: Step 1 is as follows: A polycation electrolyte solution with a mass fraction of 5 to 30 wt% is added to a polyanion electrolyte solution with a mass fraction of 5 to 30 wt%, the pH of the mixed solution is adjusted to 5 to 9, magnetic stirring is performed to fully mix the mixed solution, and the mixed solution is immediately immersed in liquid nitrogen for 10 to 60 minutes, freeze-dried to remove excess water, ground and sieved through a 200 to 2000 mesh sieve, and the particle size distribution is controlled to be 0.0002 to 0.075 mm, so as to obtain a polyelectrolyte adhesive powder.

4. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 3, characterized in that: The volume ratio of the polycation electrolyte solution to the polyanion electrolyte solution is 1-9:9-1.

5. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: The gravel in step 2 is obtained by passing industrial grade gravel through a 8-80 mesh sieve.

6. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: In step 3, industrial-grade silicate cement is sieved and graded using 250-8000 meshes to obtain silicate cement.

7. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: In step 3, the silicate cement is composed of tricalcium silicate, dicalcium silicate, tricalcium aluminate, tetracalcium aluminoferrite and gypsum in a mass ratio of 50-70:15-30:5-10:5-10:3-5.

8. The method for preparing the underwater rapid anti-seepage and long-term reinforcement plugging material according to claim 1, characterized in that: Step 4 is as follows: The polyelectrolyte adhesive powder, gravel and silicate cement in a mass ratio of 1:1-4:2-4 are evenly mixed by ball milling to obtain the plugging material.

9. Underwater rapid anti-seepage and long-term reinforcement plugging material, characterized in that: The compound is prepared by the preparation method described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Polyion complex / PVA composite slurry for flowing water plugging, and preparation method thereof

    CN109265886A

  • Underwater concrete composition and artificial reef using the same

    KR1020130130309A

  • Cement mortar composite with excellent workability and water resistance, repair method of concrete structure, injection repair method for the concrete structure, surface treating method of the concrete structure and surface protection method of the concrete structure using the composite

    KR102088407B1

  • Method for Fluid Loss Control with Two Treatment Fluids

    US20230407162A1

  • Quick setting aqueous composition comprising polyelectrolyte coacervates and polyphenols

    WO2024003041A1

Cited By

  • Rapid gelling type full-solid-waste double-liquid synchronous grouting material and preparation method thereof