Low-carbon high-toughness cement-based composite material as well as preparation method and application thereof

Through the preparation of low-carbon and high-toughness cement-based composite materials, combined with nano-complex salt crystals and ultra-high molecular weight polyethylene fibers, the shortcomings of pallet materials in terms of load-bearing capacity, environmental protection and carbon emissions are solved, and high strength, toughness and convenience are achieved. Mobile pallet materials meet the needs of low carbon and high cost performance.

CN118754584APending Publication Date: 2024-10-11CHANGZHOU ARCHITECTUAL RES INST GRP CO LTD +1

Patent Information

Application Number
CN202410777017.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing pallet materials such as steel, plastic and wooden pallets have shortcomings in terms of load-bearing capacity, environmental protection, cost and carbon emissions, and are difficult to meet the needs of low carbon, high toughness and convenient movement.

Method used

Using low-carbon and high-toughness cement-based composite materials, nano-diameter needle rod-shaped double salt crystals and closely packed hydrated calcium silicate gel are formed through the four-coordination isomerization effect and double salt effect of silicon, combined with ultra-high molecular weight polyethylene Fibers and high-strength hollow glass microbeads are used to prepare pallet materials with high strength, toughness and durability, and rebars and universal wheels are built into the main body of the pallet for convenient movement.

Benefits of technology

It achieves the high strength, toughness and durability of low-carbon and high-toughness cement-based composite pallets, reduces carbon emissions, is low-cost and highly cost-effective, and can be moved in a flat state without a forklift. It is easy to use, saves labor, time and effort. , and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754584A_ABST
    Figure CN118754584A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and discloses a low-carbon high-toughness cement-based composite material as well as a preparation method and application thereof. The low-carbon high-toughness cement-based composite material is prepared from 93.7 to 103 parts of powder, 0.8 to 1.1 parts of ultra-high molecular weight polyethylene fiber, 0.1 part of a defoaming agent, 0.1 part of a water reducing agent and 20 parts of water, wherein the powder material comprises 29-31 parts of a low-carbon cementing material, 35-39 parts of modified high-activity micro powder, 3 parts of an expanding agent, 4-7 parts of high-strength hollow glass beads and 22.7-23 parts of spherical quartz sand. The low-carbon high-toughness cement-based composite material disclosed by the invention has excellent performances in the aspects of durability such as carbonization resistance, chloride ion permeation resistance, freezing and thawing resistance, shrinkage and the like. According to the low-carbon high-toughness cement-based composite material tray, the tray main body is high in strength, toughness, durability and ductility, can replace a steel tray panel, is low in cost and high in cost performance, is provided with the universal wheels, can be moved at will without the help of a forklift in a plane state, is convenient to use, saves labor and time, and is low-carbon and environment-friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of building materials, in particular to a low-carbon high-toughness cement-based composite material and a preparation method and application thereof. Background Art

[0002] With the rapid development of the logistics industry, pallets are an important carrier in the logistics process. Their quality and performance are crucial to improving logistics efficiency and reducing costs. At present, the mainstream pallet materials on the market are steel, plastic and wood. Steel pallets have the strongest load-bearing capacity, but steel is easy to corrode, the most expensive, the heaviest, difficult to move in a flat state, and high carbon emissions; plastic pallets have moderate load-bearing capacity, but plastic is easy to age, not environmentally friendly, expensive, and high carbon emissions; although wooden pallets are cheap, wood has the lowest load-bearing capacity and is easy to break. Summary of the invention

[0003] The technical problem to be solved by the present invention is: to overcome the deficiencies in the prior art and to provide a low-carbon and high-toughness cement-based composite material and a preparation method and application thereof. The low-carbon and high-toughness cement-based composite material pallet of the present invention has high pallet main body strength, toughness, durability and elongation, can replace steel pallet panels, has low cost and high cost performance, is equipped with universal wheels, can be moved at will in a flat state without the aid of a forklift, is easy to use, saves labor, time and effort, and is low-carbon and environmentally friendly.

[0004] The technical solution adopted by the present invention to solve its technical problem is:

[0005] A low-carbon high-toughness cement-based composite material, comprising the following raw materials in parts by weight:

[0006]

[0007]

[0008] Wherein, the powder comprises the following raw materials in parts by weight:

[0009]

[0010] Furthermore, the low-carbon cementitious material is prepared from 43wt% of slag, 22wt% of magnesium slag, 15wt% of slag, 16wt% of desulfurized gypsum, 2wt% of aluminum sulfate, 1wt% of quicklime and 1wt% of potassium alum.

[0011] Low-carbon cementitious materials have the following characteristics: mechanical properties exceeding those of ordinary Portland cement 52.5, carbon emissions 75% lower than 52.5 ordinary Portland cement, and shrinkage value 50% of that; its principle is that through the "tetra-coordination isomorphism effect of silicon" and "complex salt effect", while forming a large number of nano-diameter needle-rod-shaped complex salt crystals, a large number of nearly amorphous and tightly packed hydrated calcium silicate gels and zeolite-like phases are also formed, and the needle-rod-shaped complex salt crystals are tightly wrapped, so that the entire cementitious system has good density, strength, volume stability and resistance to environmental erosion.

[0012] Furthermore, the specific surface area of ​​the low-carbon cementitious material is 550 m 2 / kg, the compressive strength after 3 days is 31Mpa, the compressive strength after 7 days is 44Mpa, and the compressive strength after 28 days is 66Mpa.

[0013] Furthermore, the modified high-activity micropowder is prepared from 86wt% fly ash, 10wt% fluorgypsum, 2wt% sodium carbonate and 2wt% sodium lactate, with a 7d activity index of 83% and a 28d activity index of 109%.

[0014] Furthermore, the particle size D90 of the high-strength hollow glass microspheres is 55 microns and the true density is 600 kg / m 3 , the compressive strength is 97MPa.

[0015] Furthermore, the ultra-high molecular weight polyethylene fiber has a molecular weight of 10 million, a length of 22 m, a diameter of 2.2D, a modulus of 1700 cN / dtex, a breaking strength of 44 cN / dtex, and a breaking elongation of 3.5%.

[0016] Furthermore, the spherical quartz sand has a particle size of 30 to 100 meshes and a roundness of 0.88; the defoaming agent is a powdered silicon defoaming agent, and the water reducing agent is a powdered polycarboxylic acid water reducing agent.

[0017] A method for preparing the low-carbon high-toughness cement-based composite material as described above specifically comprises the following steps:

[0018] Step S1, grinding the raw materials required for low-carbon gelling material and modified high-activity micropowder respectively with a planetary ball mill, and obtaining low-carbon gelling material and modified high-activity micropowder respectively after ball milling for 30 minutes;

[0019] Step S2, mixing low-carbon gelling material, modified high-activity micropowder, expansion agent, spherical quartz sand, high-strength hollow glass microspheres, defoamer and water reducing agent in proportion to prepare a mixed material;

[0020] Step S3, weighing water and ultra-high molecular weight polyethylene fibers, adding the ultra-high molecular weight polyethylene fibers into the water, and then adding the mixed material obtained in step S2, and stirring at high speed for 5 minutes to obtain a finished low-carbon high-toughness cement-based composite material.

[0021] An application of the low-carbon and high-toughness cement-based composite material as described above, wherein the low-carbon and high-toughness cement-based composite material is applied in a low-carbon and high-toughness cement-based composite material pallet.

[0022] Furthermore, the low-carbon and high-toughness cement-based composite material pallet includes a pallet body made of low-carbon and high-toughness cement-based composite material, the pallet body has multiple threaded steel bars distributed vertically and horizontally, and the lower surface of the pallet body is provided with multiple universal wheels.

[0023] The beneficial effects of the present invention are as follows: the present invention is reasonably designed and has the following advantages:

[0024] (1) The low-carbon high-toughness cement-based composite material of the present invention, wherein the low-carbon cementitious material forms a large number of nano-diameter needle-rod-shaped complex salt crystals through the "silicon tetracoordination isomorphism effect" and "complex salt effect", and also forms a large number of nearly amorphous tightly packed calcium silicate hydrate gel and zeolite-like phases, and tightly wraps the needle-rod-shaped complex salt crystals, so that the entire cementitious system has good density, strength, volume stability and resistance to environmental erosion. Therefore, the low-carbon high-toughness cement-based composite material of the present invention has excellent performance in terms of durability such as carbonization resistance, chloride ion penetration resistance, freeze-thaw resistance, shrinkage resistance, etc.;

[0025] (2) The preparation method of the present invention is simple to operate and suitable for large-scale production;

[0026] (3) The low-carbon and high-toughness cement-based composite material pallet of the present invention has high strength, toughness, durability and elongation of the pallet body, can replace the steel pallet panel, has low cost and high cost performance, is equipped with universal wheels, and can be moved freely in a flat state without the aid of a forklift. It is easy to use, saves labor, time and effort, and is low-carbon and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0028] Figure 1 It is a schematic structural diagram of a low-carbon and high-toughness cement-based composite material pallet of the present invention;

[0029] Figure 2 yes Figure 1 Bottom view of

[0030] In the figure: 1. Pallet body, 2. Universal wheel. DETAILED DESCRIPTION

[0031] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0032] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0033] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] A low-carbon high-toughness cement-based composite material, comprising the following raw materials in parts by weight:

[0035]

[0036] Wherein, the powder comprises the following raw materials in parts by weight:

[0037]

[0038] The low-carbon cementitious material is prepared from 43 wt% of slag, 22 wt% of Pidgeon magnesium slag, 15 wt% of slag, 16 wt% of desulfurized gypsum, 2 wt% of aluminum sulfate, 1 wt% of quicklime and 1 wt% of potassium alum.

[0039] The specific surface area of ​​low carbon cementitious material is 550m 2 / kg, the compressive strength after 3 days is 31Mpa, the compressive strength after 7 days is 44Mpa, and the compressive strength after 28 days is 66Mpa.

[0040] The modified high-activity micropowder is prepared from 86wt% of fly ash, 10wt% of fluorgypsum, 2wt% of sodium carbonate and 2wt% of sodium lactate, with a 7d activity index of 83% and a 28d activity index of 109%.

[0041] Expanding agent, manufactured by Denka of Japan, model HP-CSA;

[0042] High-strength hollow glass microspheres, particle size D90 is 55 microns, true density 600 kg / m 3 , compressive strength 97MPa, with physical water reduction effect, purchased from Shanxi Hainuo Technology Co., Ltd., model HN60HS;

[0043] The spherical quartz sand in the powder has a particle size of 30-100 meshes, a roundness of 0.88, and has a physical water reduction effect. It was purchased from Shijiazhuang Jiuyue Mineral Products Co., Ltd.

[0044] Ultra-high molecular weight polyethylene fiber, with a molecular weight of 10 million, a length of 22 m, a diameter of 2.2D, a modulus of 1700 cN / dtex, a breaking strength of 44 cN / dtex, and a breaking elongation of 3.5%, was purchased from DuPont China Group Co., Ltd. Shanghai Branch;

[0045] The defoamer is a powdered silicon defoamer purchased from BASF, model number is Vinapor DF 9010F;

[0046] The water reducer is a powdered polycarboxylic acid water reducer with a water reduction rate of 42%, purchased from Shanghai Sanrui Chemical Co., Ltd., model SD-600P.

[0047] A method for preparing the low-carbon high-toughness cement-based composite material as described above specifically comprises the following steps:

[0048] Step S1, grinding the raw materials required for low-carbon gelling material and modified high-activity micropowder respectively with a planetary ball mill, and obtaining low-carbon gelling material and modified high-activity micropowder respectively after ball milling for 30 minutes;

[0049] Step S2, mixing low-carbon gelling material, modified high-activity micropowder, expansion agent, spherical quartz sand, high-strength hollow glass microspheres, defoamer and water reducing agent in proportion to prepare a mixed material;

[0050] Step S3, weighing water and ultra-high molecular weight polyethylene fibers, adding the ultra-high molecular weight polyethylene fibers into the water, and then adding the mixed material obtained in step S2, and stirring at high speed for 5 minutes to obtain a finished low-carbon high-toughness cement-based composite material.

[0051] An application of the low-carbon and high-toughness cement-based composite material as described above, wherein the low-carbon and high-toughness cement-based composite material is applied in a low-carbon and high-toughness cement-based composite material pallet.

[0052] The low-carbon high-toughness cement-based composite material pallet comprises a pallet body 1 made of low-carbon high-toughness cement-based composite material, wherein the pallet body 1 has a plurality of threaded steel bars distributed vertically and horizontally therein, and a plurality of universal wheels 2 are arranged on the lower surface of the pallet body 1. The universal wheels 2 are universal wheels with locking function.

[0053] Example 1

[0054] A low-carbon high-toughness cement-based composite material, comprising the following raw materials in parts by weight:

[0055]

[0056]

[0057] Wherein, the powder comprises the following raw materials in parts by weight:

[0058]

[0059] A method for preparing the low-carbon high-toughness cement-based composite material as described above specifically comprises the following steps:

[0060] Step S1, grinding the raw materials required for low-carbon gelling material and modified high-activity micropowder respectively with a planetary ball mill, and obtaining low-carbon gelling material and modified high-activity micropowder respectively after ball milling for 30 minutes;

[0061] Step S2, mixing low-carbon gelling material, modified high-activity micropowder, expansion agent, spherical quartz sand, high-strength hollow glass microspheres, defoamer and water reducing agent in proportion to prepare a mixed material;

[0062] Step S3, weighing water and ultra-high molecular weight polyethylene fibers, adding the ultra-high molecular weight polyethylene fibers into the water, and then adding the mixed material obtained in step S2, and stirring at high speed for 5 minutes to obtain a finished low-carbon high-toughness cement-based composite material.

[0063] A method for manufacturing a low-carbon, high-toughness cement-based composite pallet:

[0064] Step (1), skeleton production,

[0065] First, cut 5 6mm threaded steel bars according to the length and width of the pallet, and then arrange them at equal intervals according to the length and width, weld and fix the steel frame, and then weld 9 universal wheels 2 with locking function to the steel frame, along the length and width, weld 3 on each side, and weld 1 at the center point;

[0066] Step (2), preparing a low-carbon high-toughness cement-based composite material,

[0067] The raw materials weighed in proportion are stirred evenly to obtain a slurry;

[0068] Step (3), pallet production,

[0069] Place the frame upside down into a flat pallet plastic mold, then pour the slurry into the mold until it is level, vibrate it slightly, control the thickness to 15mm, remove the mold after 1 day, and it can be used after it reaches the age.

[0070] In this low-carbon and high-toughness cement-based composite material pallet, the pallet body 1 has a thickness of 15 mm.

[0071] Example 2

[0072] The difference from Example 1 is that: a low-carbon high-toughness cement-based composite material comprises the following raw materials in parts by weight:

[0073]

[0074] Wherein, the powder comprises the following raw materials in parts by weight:

[0075]

[0076] Example 3

[0077] The difference from Example 1 is that: a low-carbon high-toughness cement-based composite material comprises the following raw materials in parts by weight:

[0078]

[0079] Wherein, the powder comprises the following raw materials in parts by weight:

[0080]

[0081]

[0082] Example 4

[0083] The difference from Example 1 is that: a low-carbon high-toughness cement-based composite material comprises the following raw materials in parts by weight:

[0084]

[0085] Wherein, the powder comprises the following raw materials in parts by weight:

[0086]

[0087] Comparative Example 1

[0088] Steel pallets on the market.

[0089] Comparative Example 2

[0090] Plastic pallets on the market.

[0091] Comparative Example 3

[0092] Wooden pallets on the market.

[0093] The pallets of Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to performance testing, wherein the failure load test method was carried out with reference to the failure load test in the steel fiber concrete manhole cover of GB 26537-2011, and the test process is shown in Table 1.

[0094] Table 1 Pallet performance test results of Examples 1 to 4 and Comparative Examples 1 to 3

[0095]

[0096] As can be seen from the above table, in Examples 1 to 4, with the increase in the content of ultra-high molecular weight polyethylene fiber and high-strength hollow glass microspheres, the mechanical properties are getting higher and higher, while the total weight is further reduced, achieving light weight and high strength, and having obvious cost-effectiveness compared to steel pallets, plastic pallets, and wooden pallets on the market.

[0097] In summary, the present invention is reasonably designed and has the following advantages:

[0098] (1) The low-carbon high-toughness cement-based composite material of the present invention, wherein the low-carbon cementitious material forms a large number of nano-diameter needle-rod-shaped complex salt crystals through the "silicon tetracoordination isomorphism effect" and "complex salt effect", and also forms a large number of nearly amorphous tightly packed calcium silicate hydrate gel and zeolite-like phases, and tightly wraps the needle-rod-shaped complex salt crystals, so that the entire cementitious system has good density, strength, volume stability and resistance to environmental erosion. Therefore, the low-carbon high-toughness cement-based composite material of the present invention has excellent performance in terms of durability such as carbonization resistance, chloride ion penetration resistance, freeze-thaw resistance, shrinkage resistance, etc.;

[0099] (2) The preparation method of the present invention is simple to operate and suitable for large-scale production;

[0100] (3) The low-carbon and high-toughness cement-based composite material pallet of the present invention has a pallet body 1 with high strength, toughness, durability and elongation, which can replace the steel pallet panel. It has low cost and high cost performance. It is equipped with universal wheels 2 and can be moved freely in a flat state without the aid of a forklift. It is easy to use, saves labor, time and effort, and is low-carbon and environmentally friendly.

[0101] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low-carbon, high-toughness cement-based composite material, characterized in that: The invention comprises the following raw materials in parts by weight: Wherein, the powder comprises the following raw materials in parts by weight:

2. A low-carbon and high-toughness cement-based composite material according to claim 1, characterized in that: The low-carbon cementitious material is prepared from 43 wt% of slag, 22 wt% of magnesium slag, 15 wt% of slag, 16 wt% of desulfurized gypsum, 2 wt% of aluminum sulfate, 1 wt% of quicklime and 1 wt% of potassium alum.

3. A low-carbon high-toughness cement-based composite material according to claim 2, characterized in that: The specific surface area of ​​the low-carbon cementitious material is 550 m 2 / kg, the compressive strength after 3 days is 31Mpa, the compressive strength after 7 days is 44Mpa, and the compressive strength after 28 days is 66Mpa.

4. The low-carbon high-toughness cement-based composite material according to claim 1, characterized in that: The modified high-activity micropowder is prepared from 86 wt% of fly ash, 10 wt% of fluorgypsum, 2 wt% of sodium carbonate and 2 wt% of sodium lactate, with a 7d activity index of 83% and a 28d activity index of 109%.

5. The low-carbon high-toughness cement-based composite material according to claim 1, characterized in that: The particle size D90 of the high-strength hollow glass microspheres is 55 microns and the true density is 600 kg / m 3 , the compressive strength is 97MPa.

6. The low-carbon and high-toughness cement-based composite material according to claim 1, characterized in that: The ultra-high molecular weight polyethylene fiber has a molecular weight of 10 million, a length of 22 m, a diameter of 2.2D, a modulus of 1700 cN / dtex, a breaking strength of 44 cN / dtex, and a breaking elongation of 3.5%.

7. The low-carbon and high-toughness cement-based composite material according to claim 1, characterized in that: The spherical quartz sand has a particle size of 30 to 100 meshes and a roundness of 0.88; the defoamer is a powdered silicon defoamer, and the water reducer is a powdered polycarboxylic acid water reducer.

8. A method for preparing a low-carbon, high-toughness cement-based composite material according to any one of claims 1 to 7, characterized in that: The specific steps include: Step S1, grinding the raw materials required for low-carbon gelling material and modified high-activity micropowder respectively with a planetary ball mill, and obtaining low-carbon gelling material and modified high-activity micropowder respectively after ball milling for 30 minutes; Step S2, mixing low-carbon gelling material, modified high-activity micropowder, expansion agent, spherical quartz sand, high-strength hollow glass microspheres, defoamer and water reducing agent in proportion to prepare a mixed material; Step S3, weighing water and ultra-high molecular weight polyethylene fibers, adding the ultra-high molecular weight polyethylene fibers into the water, and then adding the mixed material obtained in step S2, and stirring at high speed for 5 minutes to obtain a finished low-carbon high-toughness cement-based composite material.

9. An application of a low-carbon high-toughness cement-based composite material according to any one of claims 1 to 7, characterized in that: The low-carbon high-toughness cement-based composite material is used in a low-carbon high-toughness cement-based composite material pallet.

10. The low-carbon high-toughness cement-based composite material according to claim 9, characterized in that: The low-carbon high-toughness cement-based composite material pallet comprises a pallet main body (1) made of a low-carbon high-toughness cement-based composite material, the pallet main body (1) is internally provided with a plurality of threaded steel bars distributed vertically and horizontally, and a plurality of universal wheels (2) are provided on the lower surface of the pallet main body (1).

Citation Information

Patent Citations

  • High-toughness super sulfate cement and preparation method thereof

    CN111205002A

  • All-solid-waste-based high-strength mine filling cementing material and preparation method thereof

    CN115784703A

  • Low-carbon environment-friendly solid waste-based capillary crystalline material and preparation method thereof

    CN115893916A

  • Treatment method of household garbage incineration fly ash

    CN117185756A

  • Composite concrete pallet

    US20160368659A1

Cited By

  • Light UHPC-based logistics tray and preparation method thereof

    CN120535263A

  • A lightweight UHPC-based logistics pallet and its preparation method

    CN120535263B