Preparation method and application of MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating
By introducing MBM@ZIF-8@LDH nano-containers into epoxy resin coatings, the corrosion problem caused by coating micropores was solved, achieving a dual effect of passive barrier and active corrosion protection, and improving the coating's corrosion resistance and affinity with the resin.
Patent Information
- Application Number
- CN202310674750.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-06-08
AI Technical Summary
The micropores or microcracks formed during the curing process of existing epoxy resin coatings become channels for the penetration of corrosive media, leading to corrosion at the interface between the coating and the metal. Existing additives such as graphene, boron nitride, and MX materials are costly and have poor dispersibility, making them difficult to commercialize on a large scale.
MBM@ZIF-8@LDH modified epoxy resin coating was used to synthesize ZnAl-CO3-LDH by co-precipitation method, and a core-shell structure was constructed on its surface. The corrosion inhibitor MBM was loaded into ZIF-8 to form a core-shell nanocontainer, which not only improves the passive barrier performance, but also releases the corrosion inhibitor in response to the corrosion area.
It achieves long-term corrosion protection by passively blocking and actively responding to release corrosion inhibitors, thereby improving the corrosion resistance of the coating, reducing the preparation cost, and enhancing its affinity with organic resins.
Smart Images

Figure CN116716010B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solvent coatings, and specifically relates to a preparation method and application of a MBM@ZIF-8@LDH modified epoxy resin anti-corrosion coating. Background Art
[0002] Epoxy resin is widely used in the field of coatings due to its good adhesion, chemical resistance and processability. However, the micropores or microcracks formed in the curing process of epoxy resin may serve as penetration channels for corrosive media such as water, oxygen, and chloride ions, resulting in corrosion at the interface between the coating and the metal, which in turn leads to coating peeling and blistering. One way to solve this problem is to add passive fillers to improve the anti-corrosion performance of organic coatings. Many researchers have solved this problem by adding graphene, boron nitride and MX materials. Although they have outstanding physical barrier effects, they are not suitable for large-scale commercial production due to their high preparation cost, poor dispersibility, few surface functional groups and poor affinity with resins. Layered double hydroxide (LDH) is a multifunctional two-dimensional nanomaterial composed of a main layer with overlapping interlayer anions and water molecules. The synthesis process of this material is simple and the raw materials are easily available. The surface of the main layer contains a large number of hydroxyl groups, which improves the affinity for organic resins. On the other hand, the interlayer anions are connected to the main layer by electrostatic forces, and the interlayer anions are exchangeable, allowing LDH to capture corrosive media. Therefore, LDH has become a widely studied anti-corrosion material. However, the inherent microporous structure of LDH makes it susceptible to degradation. As the immersion time increases, the micropores preferentially provide diffusion pathways for oxygen and chloride ions to penetrate into the substrate. A solution to this problem is to add active fillers that can load corrosion inhibitors while sealing the micropores of LDH.
[0003] As a typical imidazolyl zeolite metal-organic framework, ZIF-8 not only has good stimulus-responsive release properties and can release corrosion inhibitors on demand, but can also be directly prepared using Zn ions on the surface of LDH and 2-methylimidazole, and form a core-shell structure with LDH.
[0004] Therefore, the present invention selects 2-mercaptobenzimidazole (MBM) as an environmentally friendly corrosion inhibitor, embeds it in situ into imidazolate zeolite framework-8 (ZIF-8) on LDH nanosheets, and prepares a new nanocontainer of MBM@ZIF-8@LDH, which can be used for epoxy coating. Summary of the invention
[0005] The present invention aims to improve the shortcomings that most existing epoxy resins are solvent-based coatings, and that micropores and microcracks generated during the curing process constitute penetration channels for corrosive media, and provides a preparation method and application of a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0006] To achieve the above object, the present invention adopts the following technical solution:
[0007] A method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating comprises the following steps:
[0008] 1) Preparation of MBM@ZIF-8@LDH:
[0009] 1-1) Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0010] Dissolve Zn(NO3)2·6H2O and Al(NO3)3·9H2O in deionized water to obtain a solution, add urea into a three-necked flask containing the solution, place the obtained mixture in an oil bath and vigorously stir for 23 to 25 hours, collect the product by centrifugation, wash it with deionized water, and dry it in vacuum to obtain ZnAl-CO3-LDH powder;
[0011] 1-2) MBM and sodium formate were dissolved in a three-necked flask filled with methanol, the above ZnAl-CO3-LDH powder was added to the three-necked flask, and magnetic stirring was performed at room temperature for 30 to 40 minutes to ensure the effective coordination of Zn ions and MBM molecules, and then 2-methylimidazole was added and placed in an oil bath for stirring and heating for 5 to 6 hours, the obtained product was centrifuged and washed with methanol, and finally, the collected product was dried under vacuum conditions for 14 to 16 hours to obtain MBM@ZIF-8@LDH;
[0012] 2) Preparation of MBM@ZIF-8@LDH modified epoxy resin anticorrosion coating
[0013] 2-1) adding MBM@ZIF-8@LDH into a mixed solvent of xylene and n-butanol, and ultrasonically dispersing for 3 to 3.5 hours to obtain a dispersion;
[0014] 2-2) Weigh the epoxy resin and add it to the dispersion, stir the resulting mixture evenly with a magnetic force, add a curing agent, and stir evenly with a magnetic force to obtain a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0015] In step 1-1), the molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 2:1, and the molar ratio of urea to NO3 - The molar ratio is 3:1.
[0016] In step 1-2), the usage ratio of MBM, sodium formate, ZnAl-CO3-LDH and 2-methylimidazole is 0.25g-1.00g:0.27g:0.50g:1.00g.
[0017] In step 1), the temperature in the oil bath is controlled at 88-92°C.
[0018] In step 1-2), the centrifugal separation conditions are a rotation speed of 800 to 1200 rpm and a time of 2 to 4 minutes.
[0019] In step 2-1), the mass ratio of xylene to n-butanol in the mixed solvent is 6.5-7.5:2.5-3.5.
[0020] In step 2-1), the usage ratio of MBM@ZIF-8@LDH to the mixed solvent is 3.8-4.2 g:1400 g.
[0021] In step 2-2), the magnetic stirring conditions are a rotation speed of 1000 to 1100 rpm and a time of 1 to 1.2 h.
[0022] In step 2-2), the curing agent is polyamide, and the mass ratio of epoxy resin to curing agent is 2:1.5-1.7.
[0023] The MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating can be used to prepare an anticorrosive coating: the anticorrosive coating is coated on the surface of a low carbon steel substrate using a coating machine, and cured at 80° C. for 2 hours and at 40° C. for 30 hours to form an anticorrosive coating.
[0024] The present invention uses 2-mercaptobenzimidazole (MBM) as an environmentally friendly corrosion inhibitor, and loads the corrosion inhibitor MBM into the ZIF-8@LDH nanocontainer, so that the MBM@ZIF-8@LDH nanocontainer has a dual role in the epoxy composite coating. Before corrosion, MBM@ZIF-8@LDH acts as a passive nanofiller to improve the barrier properties of the coating and the resistance to chloride ion penetration; after corrosion occurs, MBM@ZIF-8@LDH acts as an active anti-corrosion nanofiller, which can respond to pH changes in the local corrosion area, release MBM corrosion inhibitor, and prevent further damage to the exposed steel substrate.
[0025] The significant advantages of the present invention are:
[0026] 1. The two-dimensional material ZnAl-CO3-LDH prepared by the present invention has a simple synthesis process and readily available raw materials.
[0027] 2. Compared with other two-dimensional materials, the ZnAl-CO3-LDH used in the present invention has anion exchange properties and can capture corrosive media. At the same time, the surface of the ZnAl-CO3-LDH main layer contains a large number of hydroxyl groups, which improves the affinity to organic resins, which is not possessed by other two-dimensional materials.
[0028] 3. The present invention utilizes Zn ions on the surface of ZnAl-CO3-LDH to form ZIF-8 on its surface, and then ZIF-8 and ZnAl-CO3-LDH form a core-shell structure, thereby solving the inherent micropore defects of LDH.
[0029] 4. The present invention utilizes the load-bearing properties of ZIF-8. By orderly growing ZIF-8 on the surface of ZnAl-CO3-LDH and adding the corrosion inhibitor MBM, it not only increases the passive barrier effect, but also plays an active anti-corrosion role with the addition of the corrosion inhibitor, thereby achieving long-term corrosion protection.
[0030] 5. The ZIF-8 prepared in the present invention has good stimulus-responsive release performance and can release corrosion inhibitors on demand to prevent further damage to the exposed steel substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the XRD pattern of MBM@ZIF-8;
[0032] Figure 2 is the XRD pattern of LDH;
[0033] Figure 3 This is the XRD pattern of MBM@ZIF-8@LDH composite material. DETAILED DESCRIPTION
[0034] In order to make the content of the present invention easier to understand, the technical solution of the present invention is further described below in conjunction with specific implementation methods, but the present invention is not limited thereto.
[0035] Example 1
[0036] 1) Synthesis of MBM@ZIF-8@LDH:
[0037] 1-1) Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0038] Zn(NO3)2·6H2O and Al(NO3)3·9H2O were dissolved in deionized water at a molar ratio of 2:1. Then, urea (urea and NO3 - The resulting mixture was placed in an oil bath at 90° C. and vigorously stirred for 24 hours, collected by centrifugation, washed three times with deionized water, and dried in vacuo at 60° C. for 24 hours to obtain ZnAl-CO3-LDH powder.
[0039] 1-2) MBM (0.25 g) and sodium formate (0.27 g) were dissolved in a three-necked flask containing 70 mL of methanol. Then, ZnAl-CO3-LDH (0.5 g) was added to the above solution and magnetically stirred at room temperature (21 ± 2 ° C) for 30 min to ensure effective coordination between Zn ions and MBM molecules. Then 2-MI (1 g) was added to the mixed solution and placed in a 90 ° C oil bath and stirred and heated for 5 hours. The resulting product was centrifuged and washed with methanol 3 times. Finally, the collected product was dried at 80 ° C for 15 h under vacuum conditions to obtain MBM@ZIF-8@LDH.
[0040] 2) Preparation of MBM@ZIF-8@LDH modified epoxy resin anticorrosion coating
[0041] 2-1) Weigh 4 mg of MBM@ZIF-8@LDH and add it to 1.4 g of a mixed solvent (mass ratio of xylene: n-butanol = 7:3), and disperse it by ultrasonic for 3 hours to obtain a dispersion;
[0042] 2-2) 2 g of epoxy resin and 1.6 g of polyamide were added to the dispersion, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed, thereby obtaining MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0043] Application of anti-corrosion coating: The MBM@ZIF-8@LDH modified epoxy resin anti-corrosion coating was coated on the steel sheet substrate using a coating machine, and then the steel sheet substrate was placed in a hot air drying oven and cured at 80°C for 2h and 40°C for 30h to form a MBM@ZIF-8@LDH / EP anti-corrosion coating on the steel sheet substrate.
[0044] Example 2
[0045] 1) Synthesis of MBM@ZIF-8@LDH:
[0046] 1-1) Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0047] Zn(NO3)2·6H2O and Al(NO3)3·9H2O were dissolved in deionized water at a molar ratio of 2:1. Then, urea (urea and NO3 - The resulting mixture was placed in an oil bath at 90° C. and vigorously stirred for 24 hours, collected by centrifugation, washed three times with deionized water, and dried in vacuo at 60° C. for 24 hours to obtain ZnAl-CO3-LDH powder.
[0048] 1-2) MBM (0.5 g) and sodium formate (0.27 g) were dissolved in a three-necked flask containing 70 mL of methanol. Then, ZnAl-CO3-LDH (0.5 g) was added to the above solution and magnetically stirred for 30 min at room temperature (21 ± 2 ° C) to ensure effective coordination between Zn ions and MBM molecules. Then 2-MI (1 g) was added to the mixed solution and placed in a 90 ° C oil bath and stirred and heated for 5 hours. The resulting product was centrifuged and washed with methanol 3 times. Finally, the collected product was dried at 80 ° C for 15 h under vacuum conditions to obtain MBM@ZIF-8@LDH.
[0049] 2) Preparation of MBM@ZIF-8@LDH modified epoxy resin anticorrosion coating
[0050] 2-1) Weigh 4 mg of MBM@ZIF-8@LDH and add it to 1.4 g of a mixed solvent (mass ratio of xylene: n-butanol = 7:3), and disperse it by ultrasonic for 3 hours to obtain a dispersion;
[0051] 2-2) 2 g of epoxy resin and 1.6 g of polyamide were added to the dispersion, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed, thereby obtaining MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0052] Application of anti-corrosion coating: The MBM@ZIF-8@LDH modified epoxy resin anti-corrosion coating was coated on the steel sheet substrate using a coating machine, and then the steel sheet substrate was placed in a hot air drying oven and cured at 80°C for 2h and 40°C for 30h to form a MBM@ZIF-8@LDH / EP anti-corrosion coating on the steel sheet substrate.
[0053] Example 3
[0054] 1) Synthesis of MBM@ZIF-8@LDH:
[0055] 1-1) Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0056] Zn(NO3)2·6H2O and Al(NO3)3·9H2O were dissolved in deionized water at a molar ratio of 2:1. Then, urea (urea and NO3 - The resulting mixture was placed in an oil bath at 90° C. and vigorously stirred for 24 hours, collected by centrifugation, washed three times with deionized water, and dried in vacuo at 60° C. for 24 hours to obtain ZnAl-CO3-LDH powder.
[0057] 1-2) MBM (0.75 g) and sodium formate (0.27 g) were dissolved in a three-necked flask containing 70 mL of methanol. Then, ZnAl-CO3-LDH (0.5 g) was added to the above solution and magnetically stirred for 30 min at room temperature (21 ± 2 ° C) to ensure effective coordination between Zn ions and MBM molecules. Then 2-MI (1 g) was added to the mixed solution and placed in a 90 ° C oil bath and stirred and heated for 5 hours. The resulting product was centrifuged and washed with methanol 3 times. Finally, the collected product was dried at 80 ° C for 15 h under vacuum conditions to obtain MBM@ZIF-8@LDH.
[0058] 2) Preparation of MBM@ZIF-8@LDH modified epoxy resin anticorrosion coating
[0059] 2-1) Weigh 4 mg of MBM@ZIF-8@LDH and add it to 1.4 g of a mixed solvent (mass ratio of xylene: n-butanol = 7:3), and disperse it by ultrasonic for 3 hours to obtain a dispersion;
[0060] 2-2) 2 g of epoxy resin and 1.6 g of polyamide were added to the dispersion, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed, thereby obtaining MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0061] Application of anti-corrosion coating: The MBM@ZIF-8@LDH modified epoxy resin anti-corrosion coating was coated on the steel sheet substrate using a coating machine, and then the steel sheet substrate was placed in a hot air drying oven and cured at 80°C for 2h and 40°C for 30h to form a MBM@ZIF-8@LDH / EP anti-corrosion coating on the steel sheet substrate.
[0062] Comparative Example 1
[0063] Preparation of pure epoxy resin coating
[0064] 1) Weigh 1.4 g of mixed solvent (mass ratio of xylene: n-butanol = 7:3) and disperse by ultrasonic for 3 hours;
[0065] 2) 2 g of epoxy resin and 1.6 g of polyamide were added to the mixed solvent, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed to obtain a pure epoxy resin coating.
[0066] Application of anti-corrosion coating: The above pure epoxy resin coating is coated on the steel sheet substrate with a coating machine, and then the steel sheet substrate is placed in a hot air drying oven, cured at 80°C for 2h and 40°C for 30h to form an EP coating on the steel sheet substrate.
[0067] Comparative Example 2
[0068] 1) Synthesis of LDH:
[0069] Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0070] Zn(NO3)2·6H2O and Al(NO3)3·9H2O were dissolved in deionized water at a molar ratio of 2:1. Then, urea (urea and NO3 - The resulting mixture was placed in an oil bath at 90° C. and vigorously stirred for 24 hours, collected by centrifugation, washed three times with deionized water, and dried in vacuo at 60° C. for 24 hours to obtain ZnAl-CO3-LDH powder.
[0071] 2) Preparation of LDH modified epoxy resin anticorrosion coating
[0072] 2-1) Weigh 4 mg of LDH and add it to 1.4 g of a mixed solvent (mass ratio of xylene: n-butanol = 7:3), and disperse it by ultrasonic for 3 hours to obtain a dispersion;
[0073] 2-2) 2 g of epoxy resin and 1.6 g of polyamide were added to the dispersion, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed, thereby obtaining a LDH-modified epoxy resin anticorrosive coating.
[0074] Application of anti-corrosion coating: The above-mentioned LDH modified epoxy resin anti-corrosion coating is coated on the steel sheet substrate using a coating machine, and then the steel sheet substrate is placed in a hot air drying oven, cured at 80°C for 2h and 40°C for 30h to form an LDH / EP anti-corrosion coating on the steel sheet substrate.
[0075] Comparative Example 3
[0076] 1) Synthesis of ZIF-8@LDH:
[0077] 1-1) Synthesis of ZnAl-CO3-LDH by coprecipitation method using urea as hydrolyzing agent
[0078] Zn(NO3)2·6H2O and Al(NO3)3·9H2O were dissolved in deionized water at a molar ratio of 2:1. Then, urea (urea and NO3 - The resulting mixture was placed in an oil bath at 90° C. and vigorously stirred for 24 hours, collected by centrifugation, washed three times with deionized water, and dried in vacuo at 60° C. for 24 hours to obtain ZnAl-CO3-LDH powder.
[0079] 1-2) ZnAl-CO3-LDH (0.5 g) was added to a three-necked flask containing 70 mL of methanol and magnetically stirred at room temperature (21 ± 2 ° C) for 30 min. Then 2-MI (1 g) was added to the mixed solution and placed in a 90 ° C oil bath for 5 hours of stirring. The obtained product was centrifuged and washed with methanol three times. Finally, the collected product was dried at 80 ° C for 15 h under vacuum conditions to obtain MBM@ZIF-8@LDH.
[0080] 2) Preparation of ZIF-8@LDH modified epoxy resin anticorrosion coating
[0081] 2-1) Weigh 4 mg of ZIF-8@LDH and add it to 1.4 g of a mixed solvent (mass ratio of xylene: n-butanol = 7:3), and disperse it by ultrasonic for 3 hours to obtain a dispersion;
[0082] 2-2) 2 g of epoxy resin and 1.6 g of polyamide were added to the dispersion, and the resulting mixture was stirred at high speed and ultrasonicated for 3 hours each until it was well dispersed, thereby obtaining a ZIF-8@LDH modified epoxy resin anticorrosive coating.
[0083] Application of anti-corrosion coating: The above-mentioned ZIF-8@LDH modified epoxy resin anti-corrosion coating was coated on the steel sheet substrate using a coating machine, and then the steel sheet substrate was placed in a hot air drying oven and cured at 80°C for 2h and 40°C for 30h to form a ZIF-8@LDH / EP anti-corrosion coating on the steel sheet substrate.
[0084] Experimental example
[0085] The coatings of Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were tested for open circuit potential.
[0086] The anti-corrosion performance of the above coatings was evaluated by measuring the open circuit potential (OCP) in a 3.5% NaCl solution. It is well known that OCP is an effective method to evaluate the formation of protective corrosion products. In addition, the measurement of OCP reflects the stability of the film in a corrosive environment. The measurement results show that the OCP values of the EP coating, LDH / EP coating, ZIF-8@LDH / EP and MBM@ZIF-8@LDH / EP coating are -0.516V vs AgCl, -0.481V vs AgCl, -0.453V vs AgCl and -0.397V vsAgCl, respectively. Among them, the OCP of the MBM@ZIF-8@LDH / EP coating (-0.397V vs AgCl) is more positive than the OCP value of the EP coating (-0.516Vvs AgCl). It can be seen that the MBM@ZIF-8 / EP coating prepared by the present invention has the most effective protective ability in a corrosive environment.
[0087] Figure 1 is the XRD pattern of MBM@ZIF-8. Figure 1 It can be seen that MBM@ZIF-8 nanocrystals have strong diffraction peaks at 2θ=7.2°, 10.7°, 12.7° and 18.1°, corresponding to the (011), (002), (112) and (222) crystal planes of MBM@ZIF-8, respectively.
[0088] Figure 2 is the XRD pattern of LDH, Figure 2 It can be seen that the LDH two-dimensional material has three obvious characteristic peaks at 2θ=11.16°, 23.28° and 34.54°, corresponding to the reflections of the (003), (006) and (012) crystal planes, respectively.
[0089] Figure 3 is the XRD pattern of MBM@ZIF-8@LDH. Figure 3 It can be seen that both the characteristic peaks of MBM@ZIF-8 and the characteristic peaks of LDH are reflected in the MBM@ZIF-8@LDH composite material.
Claims
1. A method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating, characterized in that: The following steps are involved: 1) Preparation of MBM@ZIF-8@LDH: 1-1) Synthesis of ZnAl-CO3-LDH using urea as hydrolyzing agent Dissolve zinc nitrate hexahydrate and aluminum nitrate nonahydrate in deionized water to obtain a solution, add urea into a three-necked flask containing the solution, place the obtained mixture in an oil bath and stir for 23 to 25 hours, collect the product by centrifugation, wash and dry it, and obtain ZnAl-CO3-LDH; 1-2) MBM and sodium formate were dissolved in a three-necked flask filled with methanol, the above ZnAl-CO3-LDH was added to the three-necked flask, magnetically stirred evenly, and then 2-methylimidazole was added and placed in an oil bath for stirring and heating for 5-6 hours. The obtained product was centrifuged, washed, and dried to obtain MBM@ZIF-8@LDH; The dosage ratio of MBM, sodium formate, ZnAl-CO3-LDH, and 2-methylimidazole is 0.25g~1.00g:0.27g:0.50g:1.00g; 2) Preparation of MBM@ZIF-8@LDH modified epoxy resin anticorrosion coating 2-1) Add MBM@ZIF-8@LDH into a mixed solvent of xylene and n-butanol, and disperse by ultrasonic for 3-3.5 hours to obtain a dispersion; 2-2) Weigh the epoxy resin and add it to the dispersion, stir the mixture evenly with a magnetic force, add the curing agent, and stir evenly with a magnetic force to obtain the MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating.
2. The method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating according to claim 1, characterized in that: The molar ratio of zinc nitrate hexahydrate to aluminum nitrate nonahydrate is 2:1, and the molar ratio of urea to NO3 - The molar ratio is 3:
1.
3. The method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating according to claim 1, characterized in that: In step 1), the temperature in the oil bath is controlled at 88-92°C.
4. The method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating according to claim 1, characterized in that: In step 2-1), the mass ratio of xylene to n-butanol in the mixed solvent is 6.5-7.5:2.5-3.
5.
5. The method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating according to claim 1, characterized in that: In step 2-1), the usage ratio of MBM@ZIF-8@LDH to the mixed solvent is 3.8~4.2g:1400g.
6. The method for preparing a MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating according to claim 1, characterized in that: In step 2-2), the magnetic stirring conditions are a rotation speed of 1000-1100 rpm and a time of 1-1.2 h; the curing agent is polyamide, and the mass ratio of epoxy resin to curing agent is 2:1.5-1.
7.
7. A MBM@ZIF-8@LDH modified epoxy resin anticorrosive coating obtained according to the preparation method according to any one of claims 1 to 6.
8. The use of the anticorrosive coating according to claim 7, characterized in that: The BM@ZIF-8@LDH modified epoxy resin anti-corrosion coating is coated on the surface of the substrate and cured to form an anti-corrosion coating.
Citation Information
Patent Citations
Preparation method of high-corrosion-resistance modified epoxy resin composite coating
CN112341900A
Preparation method and application of polypyrrole-coated ZIF-8 modified epoxy resin anticorrosive paint
CN114591671A
Ti3C2Tx and ZnAl-MoO4 LDH composite corrosion inhibitor and preparation method and composite coating thereof
CN114958056A
Dual self-repairing anticorrosive coating and preparation method thereof
CN115433478A