Liquid silicone rubber as well as preparation method and application thereof
By introducing side vinyl and phenylene into the silicon oxygen main chain of liquid silicon rubber, polymerization technology is used to improve its high temperature and aging resistance, and solve the problem of insufficient tolerance of existing liquid silicon rubber in extreme environments. , achieving excellent mechanical and ceramicization properties.
Patent Information
- Application Number
- CN202411365083.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The existing liquid silicone rubber has poor tolerance in high temperature environments and has limited aging resistance, making it difficult to meet the needs of extreme environments.
By introducing pendant vinyl and phenylene groups into the silicon oxygen main chain of liquid silicon rubber, and using anionic ring-opening polymerization and condensation polymerization technology, phenylene high vinyl polysiloxane is produced, which improves its high-temperature carbon residue rate and Aging resistance.
It realizes the excellent mechanical properties, high temperature resistance and aging resistance of liquid silicone rubber. It is suitable for special adhesives, sealants and coatings, and has extremely high flame retardancy and ceramicization properties.
Smart Images

Figure CN118930870A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone rubber, and in particular to liquid silicone rubber and a preparation method and application thereof. Background Art
[0002] Liquid silicone rubber has a wide range of applications and belongs to the category of room temperature vulcanized silicone rubber (RTV). It can be vulcanized into a silicone elastomer by mixing with air or a crosslinking agent at room temperature or under slight heating. In recent years, as the working environment of materials has become increasingly harsh and materials have been kept warm for a long time in high-temperature working environments, the demand for the special functions of silicone rubber has become increasingly urgent. Silicone rubber has received widespread attention for its unique high and low temperature resistance, but common liquid silicone rubber has limited high temperature resistance and aging resistance, and has poor tolerance to extreme environments.
[0003] Therefore, it is urgent to further improve its performance. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a liquid silicone rubber and a preparation method and application thereof.
[0005] In order to achieve the above object, the present invention provides a liquid silicone rubber in a first aspect, wherein the liquid silicone rubber contains a side vinyl group and a phenylene group on its siloxane main chain.
[0006] The inventors of the present invention found in the research process that the introduction of vinyl can significantly improve the high-temperature carbon residue rate of silicone rubber, but because the vinyl can undergo cross-linking reaction at a relatively low temperature, it is not conducive to its aging resistance. The present invention introduces vinyl and phenylene into the main chain of silicon oxygen through anionic ring-opening polymerization and condensation polymerization to obtain phenylene high vinyl polysiloxane, which makes the liquid silicone rubber have excellent high temperature resistance and aging resistance, and expands its application field.
[0007] The second aspect of the present invention provides a method for preparing the liquid silicone rubber according to the first aspect, wherein the method comprises: in the presence of an initiator, polymerizing methylvinylcyclosiloxane and phenylene monomer to obtain the liquid rubber.
[0008] The third aspect of the present invention provides liquid silicone rubber obtained by the preparation method described in the second aspect.
[0009] The fourth aspect of the present invention provides the use of the liquid silicone rubber described in the first aspect or the third aspect in the preparation of special adhesives, sealants and coatings with high temperature resistance, ablation resistance and ceramicization functions.
[0010] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0011] (1) The liquid silicone rubber provided by the present invention introduces vinyl groups in the side groups and introduces phenylene groups in the main chain. Under the synergistic effect of the phenylene groups and the side vinyl groups, the liquid silicone rubber simultaneously exhibits excellent mechanical properties, high temperature resistance and aging resistance.
[0012] (2) The preparation method of the liquid silicone rubber provided by the present invention has readily available raw materials, a simple synthesis process, no need to use a reaction solvent, simple post-treatment, and the initiator used is easy to remove.
[0013] (3) The liquid silicone rubber provided by the present invention has good application effect. The ceramic silicone sealant prepared by adding ceramic filler into the liquid silicone rubber has excellent ceramic performance, especially extremely high flame retardancy (limiting oxygen index ≥46%). BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a graph showing the infrared spectrum (FT-IR) test results of the liquid silicone rubber prepared in Example 1 and Comparative Example 2 of the present invention, wherein A is the liquid silicone rubber prepared in Comparative Example 2, and B is the liquid silicone rubber prepared in Example 1. DETAILED DESCRIPTION
[0015] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0016] A first aspect of the present invention provides a liquid silicone rubber, wherein the liquid silicone rubber contains a side vinyl group and a phenylene group on its siloxane main chain.
[0017] The liquid silicone rubber provided by the present invention introduces vinyl groups in the side groups, introduces phenylene groups in the main chain, and the terminal groups are silanol groups. The terminal silanol groups give the silicone rubber good cross-linking reactivity, and a room temperature cross-linking vulcanization reaction based on a condensation polymerization mechanism can occur under the action of a cross-linking agent and a catalyst, thereby achieving effective vulcanization of the silicone rubber. Both the side vinyl groups and the phenylene groups are beneficial to improving the high temperature resistance of the liquid silicone rubber, and the specific mechanism of action is as follows:
[0018] (1) The side vinyl groups do not participate in the vulcanization reaction, but undergo a secondary cross-linking reaction under high temperature, which significantly increases the cross-linking density of the silicone rubber, thereby inhibiting the main chain cyclization degradation and greatly improving the high-temperature carbon residue rate;
[0019] (2) The phenylene groups on the main chain can induce branching reactions in adjacent structures, which reduces the content of linear chains to a certain extent and also helps to increase the cross-linking density;
[0020] (3) The free radical activity of the side vinyl group is high and it is more susceptible to side group degradation reactions than the side methyl group, thus lowering the initial decomposition temperature of the silicone rubber. However, the introduction of phenylene groups successfully overcomes this shortcoming. Under the synergistic effect of phenylene groups and side vinyl groups, the silicone rubber simultaneously exhibits extremely high initial decomposition temperature, high temperature residual carbon rate, and thermal oxidation aging resistance.
[0021] In some embodiments of the present invention, the content of the side vinyl groups is 45 mol% or less, preferably 15-45 mol%, and more preferably 25 mol%. In the present invention, if the content of the side vinyl groups is too low, the active centers of the secondary crosslinking reaction at high temperature will be reduced, the crosslinking density will not be high, and the high-temperature residual carbon rate will not be high; if the content of the side vinyl groups is too high, although the high-temperature residual carbon rate will increase, the aging resistance will be reduced.
[0022] In some embodiments of the present invention, the content of the phenylene group is less than 45 mol%, preferably 15-45 mol%, and more preferably 25-45 mol%. In the present invention, if the content of the phenylene group is too low, the improvement of the high temperature resistance and mechanical properties is not obvious; if the content of the phenylene group is too high, the improvement of the high temperature resistance has a certain limit, and it is unnecessary to have too high a content.
[0023] In some embodiments of the present invention, the liquid silicone rubber contains 0-30 mol% of phenyl groups. The phenyl groups are large in size and have a shielding effect on nearby structures. The conjugation effect of the benzene ring also enhances the bond energy of the Si-C bond, thereby helping to improve the high temperature resistance.
[0024] In the present invention, the content of each functional group can be obtained by calculation based on the raw material feed ratio, or by nuclear magnetic resonance hydrogen spectrum testing.
[0025] In some embodiments of the present invention, the liquid silicone rubber comprises a structural unit A and a structural unit B; wherein the structural unit A has a structure shown in formula (1), and the structural unit B has a structure shown in formula (2).
[0026]
[0027] In some embodiments of the present invention, the molar ratio of structural unit A to structural unit B is 5:1.5-10, preferably 5:3-9.
[0028] The above ratio can be measured by infrared spectroscopy and nuclear magnetic resonance methods, or determined based on the preparation and feeding relationship.
[0029] In some embodiments of the present invention, the liquid silicone rubber further comprises at least one of a structural unit C, a structural unit D and a structural unit E; wherein the structural unit C has a structure shown in formula (3), the structural unit D has a structure shown in formula (4), and the structural unit E has a structure shown in formula (5).
[0030]
[0031] In some embodiments of the present invention, the structural unit represented by formula (1) may be a structural unit derived from methylvinylcyclosiloxane; the structural unit represented by formula (2) may be a structural unit derived from a phenylene monomer; the structural unit represented by formula (3) may be a structural unit derived from methylcyclosiloxane; the structural unit represented by formula (4) may be a structural unit derived from methylphenylcyclosiloxane; the structural unit represented by formula (5) may be a structural unit derived from phenylcyclosiloxane.
[0032] The structural formula of the liquid silicone rubber in the present invention is shown in Formula I:
[0033]
[0034] Wherein, x, y, z, p, q are all integers, y≠0, q≠0, x, z, p can be 0;
[0035] Further,
[0036]
[0037] In some embodiments of the present invention, the number average molecular weight of the liquid silicone rubber is 40000-65000, preferably 46500-64400, and more preferably 48700-64400. In the present invention, the number average molecular weight is determined by gel permeation chromatography (GPC).
[0038] In some embodiments of the present invention, the polydispersity coefficient of the liquid silicone rubber is 1.53-1.79, preferably 1.60-1.70.
[0039] In some embodiments of the present invention, the dynamic viscosity of the liquid silicone rubber at 25° C. is 10000-25000 mPa·s, preferably 12200-14700 mPa·s, and further preferably 12200-14400 mPa·s.
[0040] The second aspect of the present invention provides a method for preparing the liquid silicone rubber according to the first aspect, wherein the method comprises: in the presence of an initiator, polymerizing methylvinylcyclosiloxane and phenylene monomer to obtain the liquid rubber.
[0041] In some embodiments of the present invention, the raw materials for the polymerization reaction further include at least one of methylcyclosiloxane, phenylcyclosiloxane and methylphenylcyclosiloxane.
[0042] In some embodiments of the present invention, the initiator is selected from at least one of tetramethylammonium hydroxide siliconate and potassium hydroxide, preferably tetramethylammonium hydroxide siliconate.
[0043] In some embodiments of the present invention, the methylvinylcyclosiloxane is selected from at least one of trimethyltrivinylcyclotrisiloxane, tetramethyltetravinylcyclotetrasiloxane and pentamethylpentavinylcyclopentasiloxane, preferably tetramethyltetravinylcyclotetrasiloxane.
[0044] In some embodiments of the present invention, the phenylene monomer is selected from at least one of 1,4-bis(dimethylhydroxysilyl)benzene and 4,4'-bis(dimethylhydroxysilyl)diphenyl ether, preferably 1,4-bis(dimethylhydroxysilyl)benzene.
[0045] In some embodiments of the present invention, the methylcyclosiloxane is selected from at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, preferably octamethylcyclotetrasiloxane.
[0046] In some embodiments of the present invention, the phenylcyclosiloxane is selected from at least one of hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane and decaphenylcyclopentasiloxane, preferably octaphenylcyclotetrasiloxane.
[0047] In some embodiments of the present invention, the methylphenylcyclosiloxane is selected from at least one of trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane and pentamethylpentaphenylcyclopentasiloxane, preferably tetramethyltetraphenylcyclotetrasiloxane.
[0048] In some embodiments of the present invention, the polymerization temperature is 90-120°C, preferably 110°C.
[0049] In some embodiments of the present invention, the polymerization time is 3-10 h, preferably 3 h.
[0050] In some embodiments of the present invention, after the polymerization reaction is completed, post-treatment is performed to obtain the liquid silicone rubber.
[0051] In some embodiments of the present invention, the post-treatment method includes: raising the system temperature to 150°C and heating for 0.5-1h to decompose excess initiator, and continuously purging for 1-2h under N2 atmosphere for denitrification treatment; then drying at 100°C for 2-4h to further remove small molecules in the system, thereby obtaining liquid silicone rubber.
[0052] In some embodiments of the present invention, the heating time is 0.5 h, the purging time is 1 h, and the drying time is 4 h.
[0053] The third aspect of the present invention provides liquid silicone rubber obtained by the preparation method described in the second aspect.
[0054] The fourth aspect of the present invention provides the use of the liquid silicone rubber described in the first aspect or the third aspect in the preparation of special adhesives, sealants and coatings with high temperature resistance, ablation resistance and ceramicization functions.
[0055] The present invention will be described in detail below through examples.
[0056] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.
[0057] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0058] The sources of raw materials in the embodiments and comparative examples of the present invention are as follows:
[0059] Tetramethylammonium hydroxide pentahydrate: purchased from J&K, CAS No. 10424-65-4;
[0060] Octamethylcyclotetrasiloxane: purchased from McLean, CAS number 556-67-2;
[0061] Tetramethyltetravinylcyclotetrasiloxane: purchased from MacLean, CAS number 2554-06-5;
[0062] Octaphenylcyclotetrasiloxane: purchased from Maclean, CAS number 546-56-5;
[0063] Tetramethyltetraphenylcyclotetrasiloxane: purchased from MacLean, CAS number 77-63-4;
[0064] 1,4-Bis(dimethylhydroxysilyl)benzene: purchased from J&K, CAS No. 2754-32-7;
[0065] Fumed silica: R8200, purchased from Evonik Degussa, CAS No. 68909-20-6;
[0066] Tetraethyl orthosilicate: purchased from McLean, CAS number is 78-10-4;
[0067] Dibutyltin dilaurate: purchased from Maclean, CAS number 77-58-7;
[0068] Composite ceramic powder: purchased from Xiangtan Youhe New Materials, brand name YH-8103;
[0069] 108 silicone rubber: phenyl content is 15 mol%, purchased from Guangzhou Laiso Chemical Technology Co., Ltd.
[0070] The initiators used in the following examples and comparative examples were prepared by the following method:
[0071] 20g of octamethylcyclotetrasiloxane and 0.4g of tetramethylammonium hydroxide pentahydrate were placed in a 100mL flask and reacted for 4h at 80°C and a vacuum degree of -0.009MPa to obtain 2% tetramethylammonium hydroxide siliconate, which is the initiator required for the polymerization reaction.
[0072] Example 1
[0073] This example is used to illustrate the preparation of liquid silicone rubber.
[0074] 17.80g (60mmol) of octamethylcyclotetrasiloxane and 8.62g (25mmol) of tetramethyltetravinylcyclotetrasiloxane were treated for dehydration at 60°C and vacuum degree of -0.09MPa for 0.5h; 0.35g of initiator and 3.40g (15mmol) of 1,4-bis (dimethylhydroxysilyl) benzene were added, the temperature was raised to 110°C, and the polymerization reaction was carried out for 3h. After the reaction, the system temperature was raised to 150°C and heated for 0.5h to decompose the excess initiator, and the system was continuously purged for 1h under nitrogen atmosphere for dehydration treatment; finally, the obtained silica gel was placed in a vacuum oven at 100°C and dried for 4h to further remove small molecules in the system, and the target product liquid silicone rubber was obtained.
[0075] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 15 mol%.
[0076] Example 2
[0077] Liquid silicone rubber was prepared according to the method of Example 1, except that the temperature of the reaction system was 120°C.
[0078] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 15 mol%.
[0079] Example 3
[0080] Liquid silicone rubber was prepared according to the method of Example 1, except that the temperature of the reaction system was 100°C.
[0081] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 15 mol%.
[0082] Example 4
[0083] Liquid silicone rubber was prepared according to the method of Example 1, except that the temperature of the reaction system was 90°C.
[0084] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 15 mol%.
[0085] Example 5
[0086] Liquid silicone rubber was prepared according to the method of Example 1, except that 5.66 g (25 mmol) of 1,4-bis(dimethylhydroxysilyl)benzene and 14.83 g (50 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0087] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 25 mol%.
[0088] Example 6
[0089] Liquid silicone rubber was prepared according to the method of Example 1, except that 7.92 g (35 mmol) of 1,4-bis(dimethylhydroxysilyl)benzene and 11.87 g (40 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0090] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 35 mol%.
[0091] Example 7
[0092] Liquid silicone rubber was prepared according to the method of Example 1, except that 10.18 g (45 mmol) of 1,4-bis(dimethylhydroxysilyl)benzene and 8.90 g (30 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0093] The liquid silicone rubber has a vinyl content of 25 mol% and a phenylene content of 45 mol%.
[0094] Example 8
[0095] Liquid silicone rubber was prepared according to the method of Example 1, except that 5.17 g (15 mmol) of tetramethyltetravinylcyclotetrasiloxane, 3.40 g (15 mmol) of 1,4-bis(dimethylhydroxysilyl)benzene and 20.76 g (70 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0096] The liquid silicone rubber has a vinyl content of 15 mol% and a phenylene content of 15 mol%.
[0097] Example 9
[0098] Liquid silicone rubber was prepared according to the method of Example 8, except that 12.07 g (35 mmol) of tetramethyltetravinylcyclotetrasiloxane and 14.83 g (50 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0099] The liquid silicone rubber has a vinyl content of 35 mol% and a phenylene content of 15 mol%.
[0100] Example 10
[0101] Liquid silicone rubber was prepared according to the method of Example 8, except that 15.52 g (45 mmol) of tetramethyltetravinylcyclotetrasiloxane and 11.86 g (40 mmol) of octamethylcyclotetrasiloxane were added to the reaction system.
[0102] The liquid silicone rubber has a vinyl content of 45 mol% and a phenylene content of 15 mol%.
[0103] Comparative Example 1
[0104] Take 108 silicone rubber as comparison.
[0105] Comparative Example 2
[0106] 44.49 g (150 mmol) of octamethylcyclotetrasiloxane and 21.54 g (62.5 mmol) of tetramethyltetravinylcyclotetrasiloxane were added to a 250 mL flask, and dewatering was performed at 60 ° C and a vacuum degree of -0.09 MPa for 0.5 h; then 0.9 g of initiator and 20.43 g (37.5 mmol) of tetramethyltetraphenylcyclotetrasiloxane were added, the temperature was raised to 120 ° C, and the polymerization reaction was carried out until the viscosity of the system increased, and 0.25 g of deionized water was added, and the reaction time was 2 h; after the reaction was completed, the system temperature was raised to 150 ° C and kept warm for 0.5 h to decompose the excess initiator; the nitrogen atmosphere was continuously purged for 1 h for denitrification treatment; finally, the silica gel obtained after the reaction was completed was placed in a 100 ° C vacuum oven for 4 h to further remove small molecules in the system, and liquid silicone rubber was obtained.
[0107] The liquid silicone rubber has a vinyl content of 25 mol % and a phenyl content of 15 mol %.
[0108] Application Example 1
[0109] This application example provides a method for preparing a ceramic organic silicon sealant using the liquid silicone rubber prepared in Example 1 as a base glue.
[0110] 120 parts of ceramic powder were added to 100 parts of the liquid silicone rubber prepared in Example 1, and after premixing, 3 parts of tetraethyl orthosilicate and 0.5 parts of dibutyltin dilaurate were added in sequence, and then further mixed on a three-roll mill. The mixture was extruded into a sheet in a flat vulcanizer, and then cured in a constant temperature and humidity chamber under standard conditions (temperature 23°C ± 2°C, relative humidity 50% ± 5%) for 7 days to obtain a ceramic silicone sealant sample.
[0111] Application Comparative Example 1
[0112] A ceramic organic silicon sealant was prepared according to the method of Application Example 1, except that the 108 silicone rubber of Comparative Example 1 was used as the base glue.
[0113] Application Comparative Example 2
[0114] A ceramic organic silicon sealant was prepared according to the method of Application Example 1, except that the liquid silicone rubber prepared in Comparative Example 2 was used as the base glue.
[0115] Effect Example 1
[0116] Yield calculation formula:
[0117] Where m1 is the total mass of the reactants before the reaction; m2 is the mass of the products after the reaction.
[0118] The number average molecular weight (Mn) and polydispersity index (PDI) of the products in Examples 1-10 and Comparative Example 2 were determined by gel permeation chromatography (GPC).
[0119] The dynamic viscosity of the products in Examples 1-10 and Comparative Example 2 was tested using a rotational viscometer.
[0120] The test results are shown in Table 1.
[0121] Table 1
[0122]
[0123] Effect Example 2
[0124] Take the liquid silicone rubber obtained in Examples 1-10 and Comparative Example 2 and the 108 silicone rubber in Comparative Example 1 as the base rubber, add 10 parts of fumed silica to 100 parts of the base rubber, add 3 parts of ethyl orthosilicate and 0.5 parts of dibutyltin disilicate after premixing, and further mix evenly on a three-roll grinder. Then extrude into sheets in a flat vulcanizer, and then cure in a constant temperature and humidity chamber under standard conditions (temperature 23°C ± 2°C, relative humidity 50% ± 5%) for 7 days to obtain a cured product.
[0125] The tensile properties were tested using a universal testing machine from Meters Industrial Systems (China) Co., Ltd. According to the provisions of GB / T528-2009, a type 3 dumbbell specimen standard was selected, the tensile rate was 200 mm / min, and the test environment was room temperature (25±2°C); according to the provisions of GB / T 531.1-2008, a Shore A durometer was used to test the hardness.
[0126] The test results are shown in Table 2.
[0127] Table 2
[0128]
[0129] From the results in Table 2, it can be seen that the introduction of phenylene groups into the main chain can significantly improve the mechanical properties of silicone rubber, and as the phenylene content increases, the mechanical properties gradually increase.
[0130] Effect Example 3
[0131] Thermogravimetric analysis (TGA) was used to measure the initial decomposition temperature, maximum decomposition temperature and high-temperature carbon residue rate of all the cured products in Example 2. The test conditions were 0-1000° C., 10° C. / min (nitrogen atmosphere).
[0132] The test results are shown in Table 3.
[0133] Table 3
[0134]
[0135] It can be seen from the above results that the liquid silicone rubber provided by the present invention has an extremely high carbon residue rate at high temperatures. When phenylene groups are introduced into the main chain, the initial decomposition temperature of the liquid silicone rubber is significantly improved, thereby obtaining excellent high temperature resistance.
[0136] Effect Example 4
[0137] The high temperature heating rapid aging method was used to measure the aging resistance of all the cured products in Example 2. The test conditions were heating at 150° C. for 48 h, 96 h and 144 h.
[0138] m1 is the mass before aging, and m2 is the mass after aging.
[0139] The test results are shown in Table 4.
[0140] Table 4
[0141]
[0142]
[0143] From the above results, it can be seen that the presence of phenylene can significantly improve the aging resistance of silicone rubber.
[0144] Effect Example 5
[0145] The ceramic silicone sealants prepared in Application Example 1 and Application Comparative Examples 1-2 were tested using a thermal gravimetric analysis (TGA), a limiting oxygen index tester, and a vertical combustion tester.
[0146] The tensile properties were tested using a universal testing machine from Meters Industrial Systems (China) Co., Ltd. According to the provisions of GB / T528-2009, a type 3 dumbbell specimen standard was selected, the tensile rate was 200 mm / min, and the test environment was room temperature (25±2°C); according to the provisions of GB / T 531.1-2008, a Shore A durometer was used to test the hardness.
[0147] The porcelain forming condition is ablation at 1000℃ for 30min, m1 is the mass before ablation, and m2 is the mass after ablation.
[0148] The test results are shown in Table 5.
[0149] Table 5
[0150]
[0151] From the above results, it can be seen that the introduction of vinyl and phenylene groups can significantly improve the ceramicization rate of silicone rubber and the thermal stability of ceramic silicone rubber. Therefore, this is beneficial to the application of ceramic silicone sealants.
[0152] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A liquid silicone rubber, characterized in that: The liquid silicone rubber contains pendant vinyl groups and phenylene groups on its siloxane main chain.
2. The liquid silicone rubber according to claim 1, wherein The content of the side vinyl groups is 45 mol% or less, preferably 15-45 mol%, and more preferably 25 mol%; Preferably, the content of the phenylene group is 45 mol% or less, preferably 15-45 mol%, and more preferably 25-45 mol%; Preferably, the liquid silicone rubber contains 0-30 mol % of pendant phenyl groups.
3. The liquid silicone rubber according to claim 1 or 2, wherein: The liquid silicone rubber comprises a structural unit A and a structural unit B; wherein the structural unit A has a structure shown in formula (1), and the structural unit B has a structure shown in formula (2). Preferably, the molar ratio of structural unit A to structural unit B is 5:1.5-10, preferably 5:3-9.
4. The liquid silicone rubber according to any one of claims 1 to 3, wherein The liquid silicone rubber further comprises at least one of a structural unit C, a structural unit D and a structural unit E; wherein the structural unit C has a structure shown in formula (3), the structural unit D has a structure shown in formula (4), and the structural unit E has a structure shown in formula (5).
5. The liquid silicone rubber according to any one of claims 1 to 4, wherein The number average molecular weight of the liquid silicone rubber is 40000-65000, preferably 46500-64400, and more preferably 48700-64400; Preferably, the polydispersity coefficient of the liquid silicone rubber is 1.53-1.79, preferably 1.60-1.70; Preferably, the dynamic viscosity of the liquid silicone rubber at 25° C. is 10000-25000 mPa·s, preferably 12200-14700 mPa·s, and further preferably 12200-14400 mPa·s.
6. A method for preparing liquid silicone rubber according to any one of claims 1 to 5, characterized in that: The method comprises: in the presence of an initiator, polymerizing methylvinyl cyclosiloxane and phenylene monomer to obtain the liquid rubber.
7. The method according to claim 6, wherein: The raw materials for the polymer reaction also include at least one of methylcyclosiloxane, phenylcyclosiloxane and methylphenylcyclosiloxane; Preferably, the initiator is selected from at least one of tetramethylammonium hydroxide siliconate and potassium hydroxide, preferably tetramethylammonium hydroxide siliconate; Preferably, the methylvinylcyclosiloxane is selected from at least one of trimethyltrivinylcyclotrisiloxane, tetramethyltetravinylcyclotetrasiloxane and pentamethylpentavinylcyclopentasiloxane, preferably tetramethyltetravinylcyclotetrasiloxane; Preferably, the phenylene monomer is selected from at least one of 1,4-bis(dimethylhydroxysilyl)benzene and 4,4'-bis(dimethylhydroxysilyl)diphenyl ether, preferably 1,4-bis(dimethylhydroxysilyl)benzene; Preferably, the methylcyclosiloxane is selected from at least one of hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, preferably octamethylcyclotetrasiloxane; Preferably, the phenylcyclosiloxane is selected from at least one of hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane and decaphenylcyclopentasiloxane, preferably octaphenylcyclotetrasiloxane; Preferably, the methylphenylcyclosiloxane is selected from at least one of trimethyltriphenylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane and pentamethylpentaphenylcyclopentasiloxane, preferably tetramethyltetraphenylcyclotetrasiloxane.
8. The method according to claim 6 or 7, wherein: The polymerization temperature is 90-120°C, preferably 110°C; Preferably, the polymerization time is 3-10 h, preferably 3 h; Preferably, after the polymerization reaction is completed, post-treatment is performed to obtain the liquid silicone rubber; Preferably, the post-treatment method comprises: raising the system temperature to 150°C and heating for 0.5-1h to decompose the excess initiator, and continuously purging for 1-2h under N2 atmosphere for denitrification treatment; then drying at 100°C for 2-4h to further remove small molecules in the system, so as to obtain liquid silicone rubber; Preferably, the heating time is 0.5 h, the purging time is 1 h, and the drying time is 4 h.
9. The liquid silicone rubber obtained by the preparation method according to any one of claims 6 to 8.
10. Use of the liquid silicone rubber according to any one of claims 1 to 5 and 9 in the preparation of special adhesives, sealants and coatings with high temperature resistance, ablation resistance and ceramicization functions.
Citation Information
Patent Citations
Damping silicon rubber with relatively small temperature effect and preparation method thereof
CN104761912A
Vinyl-terminated raw silicone rubber as well as preparation method and application thereof
CN117986586A
Room temperature-curable organopolysiloxane composition
JP2010084062A
Dynamic polymer with hybrid cross-linked network and application thereof
WO2018028365A1
Cited By
Wide-temperature-range silicone rubber base rubber for aerospace thermal protection, composite material and preparation method of wide-temperature-range silicone rubber base rubber
CN121851389A
Self-adhesive liquid silicone, preparation method and application thereof
CN122790608A