Strong-texture N-type bismuth telluride material induced by regulation and control configuration entropy and preparation method of strong-texture N-type bismuth telluride material

By regulating the configuration entropy induction and slow cooling directional solidification growth processes, the problem of texture inhomogeneity of bismuth telluride material in the zone melting method is solved, the thermoelectric properties of N-type bismuth telluride are improved, and the performance of the high-temperature section is improved and the process is simplified. , suitable for mass production.

CN118754665AActive Publication Date: 2024-10-11HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411015708.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

In the process of preparing bismuth telluride thermoelectric materials by the existing zone melting method, uneven temperature gradient results in poor texture at the head and tail of the ingot, which limits the thermoelectric performance of N-type bismuth telluride, and the process complexity and texture Non-uniformity leads to insufficient material properties.

Method used

Using the method of regulating configuration entropy induction, by adjusting the content of (Sb2Se2S) and the doping amount of BiBr3, combined with the slow cooling directional solidification growth process, N-type bismuth telluride materials with strong texture were prepared. The general chemical formula is ( Bi2Te3)1-x(Sb2Se2S)x+y at.% BiBr3, x=0.05~0.20, y=0.18~0.24, use muffle furnace for heat treatment.

Benefits of technology

It significantly improves the material's high-temperature performance, obtains a stable single-phase structure and high thermoelectric figure of merit, simplifies the process, reduces production costs, is suitable for batch preparation of large single crystals, and broadens the full-temperature range of bismuth telluride thermoelectric materials. area application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754665A_ABST
    Figure CN118754665A_ABST
Patent Text Reader

Abstract

The invention discloses a strong-texture N-type bismuth telluride material induced by regulation configuration entropy and a preparation method thereof, and belongs to the technical field of thermoelectric materials. The invention aims to solve the problems of complex process and non-uniform texture of the existing zone-melting bismuth telluride-based thermoelectric material. % BiBr3, the chemical general formula is (Bi2Te3) 1-x (Sb2Se2S) x + y at.% BiBr3, x is equal to 0.05 to 0.20, and y is equal to 0.18 to 0.24; the method comprises the following steps: 1, weighing and mixing; 2, introducing the mixed powder into a quartz ampoule bottle, and performing vacuum sealing; and 3, heating, preserving heat and cooling. The strong-texture N-type bismuth telluride material induced by the regulation and control configuration entropy and the preparation method of the strong-texture N-type bismuth telluride material are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoelectric materials. Background Art

[0002] Thermoelectric materials are functional materials that use the Seebeck effect and the Peltier effect to achieve mutual conversion between heat and electrical energy. Due to their small size, no noise, and no greenhouse gas emissions, they have been widely used in new fields such as 5G optical communications, IC refrigeration, the Internet of Things, and self-powered wearable terminals. Among the many thermoelectric material systems, bismuth telluride-based alloys and their solid solutions have become the only commercially applied thermoelectric materials due to their excellent thermoelectric properties near room temperature. However, the five-atomic layer structure of bismuth telluride determines the inherent anisotropy of bismuth telluride materials, and in N-type Bi2Te 3-x Se x In the alloy system, the conductivity in the crystallographic ab direction is 3 to 7 times that in the c-axis direction, while the thermal conductivity in the crystallographic ab direction is about 2 times that in the c-axis direction, which leads to the thermoelectric figure of merit along the ab direction being 1.5 to 2 times that in the c-axis direction. Therefore, texturing along the ab direction can clarify the direction of high thermoelectric figure of merit of the crystal, which is an indispensable requirement for optimizing the thermoelectric performance of N-type bismuth telluride. Among the many texturing strategies, the zone melting method has become one of the most commonly used methods in the industry to construct bismuth telluride texture due to its advantages such as no crucible contact, short preparation cycle and high output. However, in the process of preparing bismuth telluride by the zone melting method, the uneven temperature gradient often leads to poor texture in the region of the head and tail of the crystal rod, which accounts for about one-third of the total amount (texture degree F is less than 0.2), which greatly deteriorates the thermoelectric performance and also causes a lot of waste in production.

[0003] CN114447201A discloses a method for synthesizing bismuth telluride-based semiconductor thermoelectric materials, and the material processing process is as follows: 1) a zone melting-directional solidification vertical zone melting method assisted by induction coupling; 2) a high-density crystal nucleus rapid formation method; 3) a solid-liquid-vapor volume ratio control method modulated by argon pressure. By modulating the temperature gradient at the growth front, the temperature of the supercooled melt liquid state, and the volume ratio of the three aggregate states of solid, liquid, and vapor at the crystallization front, a nano-grain-embedded bismuth telluride-based rod-shaped thermoelectric material with a physical property non-uniformity of ≤5% along the crystal growth direction is obtained. However, its complex processing and molding process and the characteristics of insufficient texturing still largely limit the thermoelectric performance of N-type bismuth telluride. Summary of the invention

[0004] The present invention aims to solve the problems of complex process and uneven texture of existing zone-melting bismuth telluride-based thermoelectric materials, and further provide a strongly textured N-type bismuth telluride material induced by regulated configuration entropy and a preparation method thereof.

[0005] A strongly textured N-type bismuth telluride material induced by regulated configuration entropy, its chemical formula is (Bi2Te3) 1-x (Sb2Se2S) x +y at.%BiBr3; wherein x=0.05-0.20, y=0.18-0.24.

[0006] A method for preparing a strongly textured N-type bismuth telluride material induced by regulating configuration entropy is carried out according to the following steps:

[0007] 1. According to the chemical formula (Bi2Te3) 1-x (Sb2Se2S) x +y at.%BiBr3 stoichiometric ratio Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain a mixed powder; wherein x = 0.05 to 0.20, y = 0.18 to 0.24;

[0008] 2. introducing the mixed powder into a pointed-bottom quartz tube and vacuum-sealing it to obtain a sealed pointed-bottom quartz tube;

[0009] 3. Place the sealed pointed-bottom quartz tube in a muffle furnace, first keep it at 700℃~1000℃ for 2h~20h, then cool it to 400℃~650℃ at a cooling rate of 0.01℃ / min~10℃ / min, then cool it to 400℃~600℃ at a cooling rate of 0.01℃ / min~10℃ / min, and finally cool it to room temperature with the furnace to obtain a strongly textured N-type bismuth telluride material induced by regulated configurational entropy.

[0010] The beneficial effects of the present invention are:

[0011] 1. In terms of formulation, the present invention effectively expands the band gap of thermoelectric materials by adjusting the content of (Sb2Se2S), and at the same time increases the configuration entropy of the material system, thereby significantly improving the high-temperature performance of the material while obtaining a stable single-phase structure. In addition, by auxiliary adjustment of the doping amount of BiBr3 and controlling the concentration of carriers, the thermoelectric figure of merit of the material is further improved.

[0012] 2. In terms of preparation process, the present invention adopts slow cooling directional solidification growth to prepare N-type bismuth telluride material with strong texture through configuration entropy induction.

[0013] 3. The preparation process adopted by the present invention is simple and easy, with low production cost, large single tube output, no need for complex and expensive equipment, no need for human intervention in the growth process of strongly textured N-type bismuth telluride material, and good repeatability, which is suitable for batch preparation of large single crystals.

[0014] 4. Strongly textured N-type bismuth telluride material (Bi2Te3) prepared by the present invention1-x (Sb2Se2S) x +y at.%BiBr3 (x=0.05~0.20, y=0.18~0.24), through regulation, the thermoelectric figure of merit can reach 1.15 at 323K, 1.05 at 373K, or 0.95 at 473K, which broadens the full temperature range application of bismuth telluride thermoelectric materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a diagram of the heating-keeping-cooling process in the muffle furnace in step 3 of Example 1;

[0016] Figure 2 XRD images of the strongly textured N-type bismuth telluride material induced by regulated configuration entropy prepared in Example 1 along the direction perpendicular to the grain growth direction and along the direction parallel to the grain growth direction, 1 is along the direction parallel to the grain growth direction, 2 is along the direction perpendicular to the grain growth direction;

[0017] Figure 3 The backscattered diffraction (EBSD) images of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1 along the direction perpendicular to the grain growth direction and along the direction parallel to the grain growth direction, 1 is the EBSD image along the direction parallel to the grain growth direction, and 2 is the EBSD image along the direction perpendicular to the grain growth direction;

[0018] Figure 4 The macroscopic morphology of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Examples 1 to 3 and the bismuth telluride material prepared in the comparative experiment, a is the upper top surface of the bismuth telluride material prepared in the comparative experiment, b is the crystal cleaved along the van der Waals layer of the bismuth telluride material prepared in the comparative experiment, c is the upper top surface of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, d is the appearance of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, e is the crystal cleavage surface cleaved along the van der Waals layer of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, and f is the cleavage surface of the crystal cleaved along the van der Waals layer of the regulated configuration entropy prepared in Example 2. induced by the configuration entropy prepared in Example 2, g is the appearance of the strongly textured N-type bismuth telluride material induced by the control configuration entropy prepared in Example 2, h is the crystal cleavage plane cleaved along the van der Waals layer of the strongly textured N-type bismuth telluride material induced by the control configuration entropy prepared in Example 2, i is the upper top surface of the strongly textured N-type bismuth telluride material induced by the control configuration entropy prepared in Example 3, j is the longitudinal cutting surface (j-1) of the strongly textured N-type bismuth telluride material induced by the control configuration entropy prepared in Example 3, the sample obtained by cutting for thermal conductivity characterization (j-2) and the sample obtained by cutting for electrical conductivity and Seebeck coefficient characterization (j-3);

[0019] Figure 5The figure shows the relationship between the thermoelectric figure of merit and temperature of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Examples 1 to 3 and the bismuth telluride material prepared in the comparative experiment. DETAILED DESCRIPTION

[0020] Specific implementation method 1: This implementation method is a strong textured N-type bismuth telluride material induced by regulating configuration entropy, and its chemical formula is (Bi2Te3) 1-x (Sb2Se2S) x +y at.%BiBr3; wherein x=0.05-0.20, y=0.18-0.24.

[0021] The beneficial effects of this embodiment are:

[0022] 1. In terms of formulation, this embodiment effectively expands the band gap of the thermoelectric material by adjusting the content of (Sb2Se2S), and at the same time increases the configuration entropy of the material system, thereby significantly improving the high-temperature performance of the material while obtaining a stable single-phase structure. In addition, by auxiliary adjustment of the doping amount of BiBr3 and controlling the concentration of carriers, the thermoelectric figure of merit of the material is further improved.

[0023] 2. In terms of preparation process, this embodiment adopts slow cooling directional solidification growth to prepare N-type bismuth telluride material with strong texture through configuration entropy induction.

[0024] 3. The preparation process adopted in this embodiment is simple and easy, with low production cost and large single tube output. It does not require complex and expensive equipment. The growth process of strongly textured N-type bismuth telluride material does not require human intervention. The preparation process has good repeatability and is suitable for batch preparation of large single crystals.

[0025] 4. Strongly textured N-type bismuth telluride material (Bi2Te3) prepared in this embodiment 1-x (Sb2Se2S) x +y at.%BiBr3 (x=0.05~0.20, y=0.18~0.24), through regulation, the thermoelectric figure of merit can reach 1.15 at 323K, 1.05 at 373K, or 0.95 at 473K, which broadens the full temperature range application of bismuth telluride thermoelectric materials.

[0026] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that its chemical formula is (Bi2Te3) 0.95 (Sb2Se2S) 0.05 +0.18at.%BiBr3. Others are the same as those in the first embodiment.

[0027] Specific implementation method 3: This implementation method is different from the specific implementation method 1 or 2 in that its chemical formula is (Bi2Te3)0.9 (Sb2Se2S) 0.1 +0.21at.%BiBr3. Others are the same as those in the first or second embodiment.

[0028] Specific embodiment 4: This embodiment is different from the specific embodiments 1 to 3 in that its chemical formula is (Bi2Te3) 0.8 (Sb2Se2S) 0.2 +0.24at.%BiBr3. Other aspects are the same as those in the first to third embodiments.

[0029] Specific implementation method 5: This implementation method is a method for preparing a strongly textured N-type bismuth telluride material induced by regulating configuration entropy, which is carried out according to the following steps:

[0030] 1. According to the chemical formula (Bi2Te3) 1-x (Sb2Se2S) x +y at.%BiBr3 stoichiometric ratio Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain a mixed powder; wherein x = 0.05 to 0.20, y = 0.18 to 0.24;

[0031] 2. introducing the mixed powder into a pointed-bottom quartz tube and vacuum-sealing it to obtain a sealed pointed-bottom quartz tube;

[0032] 3. Place the sealed pointed-bottom quartz tube in a muffle furnace, first keep it at 700℃~1000℃ for 2h~20h, then cool it to 400℃~650℃ at a cooling rate of 0.01℃ / min~10℃ / min, then cool it to 400℃~600℃ at a cooling rate of 0.01℃ / min~10℃ / min, and finally cool it to room temperature with the furnace to obtain a strongly textured N-type bismuth telluride material induced by regulated configurational entropy.

[0033] Specific implementation example 6: This implementation example is different from specific implementation example 5 in that the purity of the Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder in step 1 are all 99.999%. The rest is the same as specific implementation example 5.

[0034] Specific embodiment 7: This embodiment is different from specific embodiment 5 or 6 in that: the particle size of the Bi particles in step 1 is 0.01mm-2mm; the particle size of the Te block in step 1 is 0.5mm-5mm; the particle size of the Se particles in step 1 is 0.01mm-2mm; the particle size of the Sb block in step 1 is 0.5mm-5mm; the particle size of the S powder in step 1 is 0.005mm-0.1mm; the particle size of the BiBr3 powder in step 1 is 0.001mm-0.1mm. The rest is the same as specific embodiment 5 or 6.

[0035] Specific implementation eight: This implementation differs from one of specific implementations five to seven in that in step three, the sealed pointed-bottom quartz tube is placed vertically on the ground in a muffle furnace. The rest is the same as specific implementations five to seven.

[0036] Specific embodiment 9: This embodiment is different from any one of specific embodiments 5 to 8 in that: in step 3, the temperature is increased to 700° C. to 1000° C. at a heating rate of 0.1° C. / min to 10° C. / min. The rest is the same as specific embodiments 5 to 8.

[0037] Specific embodiment 10: This embodiment differs from specific embodiments 5 to 9 in that: in step 3, the temperature is first raised to 800°C at a heating rate of 5°C / min, kept at 800°C for 8h, then cooled to 620°C at a cooling rate of 5°C / min, and then cooled to 550°C at a cooling rate of 0.02°C / min. The rest is the same as specific embodiments 5 to 9.

[0038] The following examples are used to verify the beneficial effects of the present invention:

[0039] Embodiment 1, combined with Figure 1 Specific instructions:

[0040] A method for preparing a strongly textured N-type bismuth telluride material induced by regulating configuration entropy is carried out according to the following steps:

[0041] 1. According to the chemical formula (Bi2Te3) 0.95 (Sb2Se2S) 0.05 +0.18at.%BiBr3 stoichiometric ratio Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain a mixed powder;

[0042] 2. introducing the mixed powder into a pointed-bottom quartz tube and vacuum-sealing it to obtain a sealed pointed-bottom quartz tube;

[0043] 3. Place the sealed pointed-bottom quartz tube vertically on the ground in a muffle furnace, first heat it to 800°C at a heating rate of 5°C / min, keep it at 800°C for 8 hours, then cool it to 620°C at a cooling rate of 5°C / min, then cool it to 550°C at a cooling rate of 0.02°C / min, and finally cool it to room temperature with the furnace to obtain a strongly textured N-type bismuth telluride material induced by regulated configurational entropy.

[0044] The purity of the Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder described in step 1 is 99.999%.

[0045] The average particle size of the Bi particles described in step one is 2 mm; the average particle size of the Te blocks described in step one is 3 mm; the average particle size of the Se particles described in step one is 2 mm; the average particle size of the Sb blocks described in step one is 1 mm; the average particle size of the S powder described in step one is 0.1 mm; the average particle size of the BiBr3 powder described in step one is 0.05 mm.

[0046] The vacuum seal pressure in step 2 is 3×10 -3 Pa.

[0047] Embodiment 2: This embodiment is different from Embodiment 1 in that: in step 1, the chemical formula is (Bi2Te3) 0.9 (Sb2Se2S) 0.1 +0.21at.%BiBr3 stoichiometric ratio Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain mixed powder. Others are the same as in Example 1.

[0048] Embodiment 3: This embodiment is different from the embodiment 1 in that: in step 1, the chemical formula is (Bi2Te3) 0.8 (Sb2Se2S) 0.2 +0.24at.%BiBr3 stoichiometric ratio Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain mixed powder. Others are the same as in Example 1.

[0049] Comparative experiment: The difference between this embodiment and the first embodiment is that in step 1, Bi particles and Te blocks are weighed and mixed according to the stoichiometric ratio of the chemical formula Bi2Te3 to obtain a mixed powder; and in step 3, bismuth telluride material is obtained. The rest is the same as the first embodiment.

[0050] Figure 2The XRD images of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1 are perpendicular to the grain growth direction and parallel to the grain growth direction. 1 is parallel to the grain growth direction, and 2 is perpendicular to the grain growth direction. It can be seen from the figure that the diffraction peaks in line 1 are (006), (0012), (0015) and (0018), all of which are (00L) crystal planes, and the orientation factor F is about 1. There are no other diffraction peaks of non-(00L) crystal planes, indicating that the organizational structure of the sample is relatively uniform and close to the single crystal level. Line 2 shows diffraction peaks such as (015) that are different from the (00L) crystal plane family, indicating that the sample may have orientation differences along the growth direction. Based on the comprehensive XRD results, the N-type bismuth telluride material prepared by this method has a high texture degree along the growth direction.

[0051] Figure 3 The backscattered diffraction (EBSD) images of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1 are perpendicular to the grain growth direction and parallel to the grain growth direction. 1 is the EBSD image along the direction parallel to the grain growth direction, and 2 is the EBSD image along the direction perpendicular to the grain growth direction. From the backscattered electron diffraction results along the direction parallel to the grain growth direction, it can be seen that the plane completely shows a single orientation composed of the (001) crystal plane, which corresponds to the XRD results. The results along the direction perpendicular to the grain growth direction show that in one area, four indices (1-100) perpendicular to the (001) crystal plane can be presented. According to the comprehensive EBSD results, the N-type bismuth telluride material prepared by this method has a high texture degree along the growth direction, close to the single crystal level.

[0052] Figure 4The macroscopic morphology of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Examples 1 to 3 and the bismuth telluride material prepared in the comparative experiment, a is the upper top surface of the bismuth telluride material prepared in the comparative experiment, b is the crystal cleaved along the van der Waals layer of the bismuth telluride material prepared in the comparative experiment, c is the upper top surface of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, d is the appearance of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, e is the crystal cleavage surface cleaved along the van der Waals layer of the strongly textured N-type bismuth telluride material induced by the regulated configuration entropy prepared in Example 1, and f is the cleavage surface of the crystal cleaved along the van der Waals layer of the regulated configuration entropy prepared in Example 2. The top surface of the induced strong texture N-type bismuth telluride material, g is the appearance of the strong texture N-type bismuth telluride material induced by the regulated configurational entropy prepared in Example 2, h is the crystal cleavage plane cleaved along the van der Waals layer of the strong texture N-type bismuth telluride material induced by the regulated configurational entropy prepared in Example 2, i is the top surface of the strong texture N-type bismuth telluride material induced by the regulated configurational entropy prepared in Example 3, j is the longitudinal cutting surface (j-1) of the strong texture N-type bismuth telluride material induced by the regulated configurational entropy prepared in Example 3, the sample obtained by cutting for thermal conductivity characterization (j-2) and the sample obtained by cutting for electrical conductivity and Seebeck coefficient characterization (j-3). As can be seen from Figure a, since the comparative experiment has not been carried out according to the present invention for element doping and configuration entropy regulation, it can be seen that a relatively chaotic organizational structure appears on the top surface of the sample; as can be seen from Figure b, although the crystals cleaved along the van der Waals layer of the bismuth telluride material prepared in the comparative experiment have a layered structure, it is difficult to obtain a complete layered crystal with good quality and large size. The layered structures of the local crystals are perpendicular to each other and there is a large misorientation angle. It can be considered that in the crystals that have not been doped with elements and regulated for configuration entropy according to the present invention, the organizational structure is relatively chaotic and the orientation is poor. Compared with Figure a, Figure c shows that the sample of Example 1 has obviously obtained a layered organization concentrated in the same direction, and the texture is significantly improved. Mirror reflection can be clearly observed from Figure e, and this mirror reflection gloss extends from the top to the bottom of the sample, achieving full coverage, which shows that the sample of Example 1 after element doping and configuration entropy regulation has obtained a high-quality layered organization with a high texture. As can be seen from Figures f, g and h, the results of Example 2 are highly similar to those of Example 1. It can be seen from the cuboid in Figure j-3 that it still has obvious mirror features, proving that Example 3 also retains a strong texture.

[0053] Figure 5The relationship between the thermoelectric figure of merit and temperature of the strongly textured N-type bismuth telluride materials induced by the configuration entropy induced by the control of Examples 1 to 3 and the bismuth telluride materials prepared by the comparative experiment. The thermoelectric figure of merit test results of all samples are characterized along the crystal growth direction; as can be seen from the figure, the thermoelectric figure of merit of the material prepared by the comparative experiment is only 0.64 at 300K due to the lack of bandgap width control and organizational structure optimization, while the strongly textured N-type bismuth telluride material induced by element doping and configuration entropy control in the embodiment has excellent thermoelectric performance, among which the sample of Example 1 reaches a thermoelectric figure of merit of 1.15 at 323K, and the peak value of the thermoelectric figure of merit of the sample of Example 2 is shifted to high temperature because the bandgap is further increased, reaching 1.05 at 373K, and the thermoelectric figure of merit of the sample of Example 3 reaches 0.95 at 473K for the same reason. The thermoelectric performance of the samples of the three embodiments is much higher than that of the materials prepared by the comparative experiment without composition control and organizational structure optimization.

Claims

1. A strongly textured N-type bismuth telluride material induced by regulated configurational entropy, characterized in that Its general chemical formula is (Bi2Te3) 1-x (Sb2Se2S) x +y at.%BiBr3; wherein x=0.05~0.20, y=0.18~0.

24.

2. The strong textured N-type bismuth telluride material induced by regulated configurational entropy according to claim 1, characterized in that Its chemical formula is (Bi2Te3) 0.95 (Sb2Se2S) 0.05 +0.18at.%BiBr3.

3. The strong textured N-type bismuth telluride material induced by regulated configurational entropy according to claim 1, characterized in that Its chemical formula is (Bi2Te3) 0.9 (Sb2Se2S) 0.1 +0.21 at.% BiBr3.

4. The strong textured N-type bismuth telluride material induced by regulated configurational entropy according to claim 1, characterized in that Its chemical formula is (Bi2Te3) 0.8 (Sb2Se2S) 0.2 +0.24at.%BiBr3.

5. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 1, characterized in that It is carried out in the following steps:

1. According to the general chemical formula (Bi2Te3) 1-x (Sb2Se2S) x +y at.% BiBr3 stoichiometric ratio: Weigh Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder and mix them to obtain a mixed powder; wherein x = 0.05 to 0.20, y = 0.18 to 0.24; 2. introducing the mixed powder into a conical-bottom quartz tube and vacuum-sealing it to obtain a sealed conical-bottom quartz tube; 3. Place the sealed pointed-bottom quartz tube in a muffle furnace, first keep it at 700℃~1000℃ for 2h~20h, then cool it to 400℃~650℃ at a cooling rate of 0.01℃ / min~10℃ / min, then cool it to 400℃~600℃ at a cooling rate of 0.01℃ / min~10℃ / min, and finally cool it to room temperature with the furnace to obtain a strongly textured N-type bismuth telluride material induced by regulated configurational entropy.

6. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 5, characterized in that The purity of the Bi particles, Te blocks, Se particles, Sb blocks, S powder and BiBr3 powder described in step 1 is 99.999%.

7. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 5, characterized in that The particle size of the Bi particles described in step one is 0.01mm~2mm; the particle size of the Te block described in step one is 0.5mm~5mm; the particle size of the Se particles described in step one is 0.01mm~2mm; the particle size of the Sb block described in step one is 0.5mm~5mm; the particle size of the S powder described in step one is 0.005mm~0.1mm; the particle size of the BiBr3 powder described in step one is 0.001mm~0.1mm.

8. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 5, characterized in that In step 3, the sealed pointed-bottom quartz tube is placed vertically on the ground in a muffle furnace.

9. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 5, characterized in that In step 3, the temperature is increased to 700° C. to 1000° C. at a heating rate of 0.1° C. / min to 10° C. / min.

10. The method for preparing a strongly textured N-type bismuth telluride material induced by regulating configurational entropy according to claim 5, characterized in that In step 3, the temperature is first increased to 800°C at a heating rate of 5°C / min, kept at 800°C for 8 hours, then cooled to 620°C at a cooling rate of 5°C / min, and then cooled to 550°C at a cooling rate of 0.02°C / min.

Citation Information

Patent Citations

  • Bi-Sb-Te-Se-S five-element high-entropy alloy and preparation method of Bi-Sb-Te-Se-S five-element high-entropy alloy

    CN111244257A

  • Preparation method of highly textured nanocrystalline bismuth telluride

    CN113774492A

  • Wide-temperature-range high-performance bismuth telluride-based thermoelectric material, preparation method and application thereof

    CN116546872A

  • N-type BiSbSe3-based thermoelectric material and preparation method and application thereof

    CN118354653A

  • Thermoelectric material and process for manufacturing the same

    US20030168094A1