Low-temperature sintered zirconia and application thereof in false tooth preparation
Through the low-temperature sintering zirconia process, the problems of high preparation cost and insufficient performance of traditional zirconia ceramics are solved, and high-density and strength zirconia ceramics are achieved, which are suitable for the preparation of various types of dentures, improving the aesthetics and application scope. .
Patent Information
- Application Number
- CN202410741998.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-11
- Publication Date
- 2024-10-11
AI Technical Summary
The traditional preparation process of zirconia ceramics requires high-temperature sintering, which results in high preparation costs and is prone to defects such as grain growth, pores and cracks, affecting its physical and chemical properties.
Using a low-temperature sintering zirconia process, zirconia powder is mixed with rare earth oxides, calcium carbonate, polyvinyl alcohol and silica in a specific proportion, and then ball-milled in an air or oxygen atmosphere, and then sintered at a low temperature. The sintering temperature is 1200-1400℃, sintering time is 1-2 hours, to produce low-temperature sintered zirconia with high density and strength.
It effectively reduces the preparation cost, increases the density and strength of zirconia, reduces defects, enhances its biocompatibility and corrosion resistance, expands the scope of application in denture preparation, and improves aesthetics and comfort. .
Abstract
Description
Technical Field
[0001] The present invention relates to the field of preparation of denture materials, and in particular to low-temperature sintered zirconium oxide and application thereof in preparation of dentures. Background Art
[0002] Dentures are medical devices used to replace missing teeth. Modern dentures are mainly composed of two parts: crowns and bridges. Crowns are used to replace a single missing tooth, while bridges are used to replace multiple missing teeth. Traditional denture preparation materials are mainly metal materials and ceramic materials. Ceramic materials have high aesthetics and biocompatibility, so they are widely used in denture preparation.
[0003] Zirconia ceramics are a commonly used ceramic material with high strength and wear resistance, and can be used to prepare high-quality dentures. However, the traditional zirconia ceramic preparation process requires high-temperature sintering, and the sintering temperature and sintering time are long, resulting in high preparation costs. In addition, traditional zirconia ceramics are prone to defects such as grain growth, pores, and cracks during the sintering process, which affects their physical and chemical properties.
[0004] Therefore, it is necessary to develop a low-temperature sintered zirconia to reduce the preparation cost while improving its physical and chemical properties to meet the needs of denture preparation. Summary of the invention
[0005] The purpose of the present invention is to provide a low-temperature sintered zirconia and its application in the preparation of dentures, and to prepare high-quality dentures by utilizing the excellent physical and chemical properties of zirconia powder. The low-temperature sintered zirconia is obtained through a specific preparation process, has high density and strength, and has a low sintering temperature and sintering time, which can effectively reduce the preparation cost.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A low-temperature sintered zirconium oxide is prepared from the following raw materials according to weight proportion: 84-90% zirconium oxide powder, 3-8% rare earth oxide, 2-5% calcium carbonate, 0.5-1.5% polyvinyl alcohol and 0.5-1.5% silicon dioxide.
[0008] As a further solution of the present invention, the low-temperature sintered zirconium oxide is prepared from the following raw materials according to weight proportion: 88% zirconium oxide powder, 6% rare earth oxide, 4% calcium carbonate, 1% polyvinyl alcohol, and 1% silicon dioxide.
[0009] As a further embodiment of the present invention, the rare earth oxide is lanthanum oxide, gadolinium oxide, or yttrium oxide.
[0010] As a further solution of the present invention, the sintering temperature of the low-temperature sintered zirconia is 1200-1400° C., and the sintering time is 1-2 hours.
[0011] As a further solution of the present invention, the rare earth oxide is further doped with a metal oxide, the metal oxide is one of zirconium oxide, silicon nitride, aluminum nitride, titanium oxide, aluminum oxide, magnesium oxide and sodium oxide, and the content of the metal oxide is 0.1-1.0wt%.
[0012] As a further embodiment of the present invention, the low temperature sintered zirconia further comprises the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0013] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol, and silicon dioxide to continue mixing, wherein the additive is a rare earth oxide composed of lanthanum oxide, gadolinium oxide, and yttrium oxide;
[0014] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 2-4 hours;
[0015] Step 3: The ball-milled powder is subjected to low-temperature sintering at a sintering temperature of 1200-1400° C. for 1-2 hours to obtain low-temperature sintered zirconia.
[0016] As a further solution of the present invention, in an oxygen atmosphere, the heating rate is 5°C / min, the sintering temperature is 1200°C, the temperature is kept for 1 hour, and then the temperature is lowered to room temperature to obtain low-temperature sintered zirconia.
[0017] As a further solution of the present invention, the density of the low-temperature sintered zirconia is greater than 98%, the strength of the low-temperature sintered zirconia is greater than 800 MPa, and the thermal expansion coefficient of the low-temperature sintered zirconia is lower than 8×10^-6 / K.
[0018] As a further solution of the present invention, the light transmittance of the low-temperature sintered zirconia is greater than 40%, and the polishability of the low-temperature sintered zirconia is less than Ra0.02 μm.
[0019] A denture prepared by using the above-mentioned low-temperature sintered zirconia, wherein the sintering temperature in the preparation process of the denture is 1200-1400°C and the sintering time is 1-2 hours.
[0020] As a further solution of the present invention, a method for preparing a denture made of low-temperature sintered zirconia is as follows: adding the ball-milled powder into a mold, pressing, sintering, and finally polishing to obtain a high-quality denture.
[0021] Compared with the prior art, the low-temperature sintered zirconia and its application in denture preparation provided by the present invention have the following beneficial effects:
[0022] 1. Reduce preparation cost: The traditional zirconia ceramic preparation process requires high-temperature sintering, and the sintering temperature and sintering time are long, and the preparation cost is high. However, the low-temperature sintered zirconia provided by the present invention has a lower sintering temperature and a shorter sintering time, which can effectively reduce the preparation cost.
[0023] 2. Improve physical and chemical properties: The low-temperature sintered zirconium oxide provided by the present invention is obtained through a specific preparation process, has high density and strength, can withstand greater pressure and impact, and has good biocompatibility and corrosion resistance.
[0024] 3. Expanding the scope of application: The low-temperature sintered zirconia provided by the present invention can be used to prepare various types of dentures, including single crowns, multiple bridges, etc., and has broad application prospects.
[0025] 4. Improve aesthetics: The low-temperature sintered zirconia provided by the present invention has high light transmittance and polishability, which can improve the aesthetics and comfort of dentures.
[0026] In summary, the low-temperature sintered zirconia provided by the present invention and its application in denture preparation have high economic and social benefits and can meet the needs of denture preparation. DETAILED DESCRIPTION
[0027] The technical solution of the present invention is further described in detail below in conjunction with specific implementation methods.
[0028] Example 1
[0029] The embodiment of the present invention provides a low-temperature sintered zirconia, which is prepared from the following raw materials in weight proportion: 89% zirconia powder, 8% rare earth oxide, 2% calcium carbonate, 0.5% polyvinyl alcohol, and 0.5% silicon dioxide.
[0030] In this embodiment, the rare earth oxide is a mixture of lanthanum oxide, gadolinium oxide, and yttrium oxide in a weight ratio of 1:1:1.
[0031] The sintering temperature of the low-temperature sintered zirconia is 1200° C., and the sintering time is 2 hours.
[0032] In this embodiment, the low temperature sintered zirconia further includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0033] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol and silicon dioxide and continue mixing;
[0034] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 2 hours;
[0035] Step 3: The ball-milled powder is subjected to low-temperature sintering, with a heating rate of 5°C / min, a sintering temperature of 1200°C, and a sintering time of 2 hours. After cooling to room temperature, low-temperature sintered zirconia is obtained.
[0036] Example 2
[0037] The embodiment of the present invention provides a low-temperature sintered zirconia, which is prepared from the following raw materials in weight proportion: 90% zirconia powder, 5.4% rare earth oxide, 3% calcium carbonate, 0.8% polyvinyl alcohol, and 0.8% silicon dioxide.
[0038] In this embodiment, the rare earth oxide is a mixture of lanthanum oxide, gadolinium oxide, and yttrium oxide in a weight ratio of 1:1:1.
[0039] The sintering temperature of the low-temperature sintered zirconia is 1250° C., and the sintering time is 1.8 hours.
[0040] In this embodiment, the low temperature sintered zirconia further includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0041] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol, and silicon dioxide to continue mixing, wherein the additive is a rare earth oxide composed of lanthanum oxide, gadolinium oxide, and yttrium oxide;
[0042] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 3 hours;
[0043] Step 3: The ball-milled powder is subjected to low-temperature sintering, with a heating rate of 5°C / min, a sintering temperature of 1250°C, and a sintering time of 1.8 hours. After cooling to room temperature, low-temperature sintered zirconia is obtained.
[0044] Example 3
[0045] The embodiment of the present invention provides a low-temperature sintered zirconia, which is prepared from the following raw materials in weight proportion: 88% zirconia powder, 7% rare earth oxide, 3% calcium carbonate, 1% polyvinyl alcohol, and 1% silicon dioxide.
[0046] In this embodiment, the rare earth oxide is a mixture of lanthanum oxide, gadolinium oxide, and yttrium oxide in a weight ratio of 1:1:1.
[0047] The sintering temperature of the low-temperature sintered zirconia is 130° C., and the sintering time is 1.5 hours.
[0048] In this embodiment, the low temperature sintered zirconia further includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0049] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol and silicon dioxide and continue mixing;
[0050] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 3 hours;
[0051] Step 3: The ball-milled powder is subjected to low-temperature sintering, with a heating rate of 5°C / min, a sintering temperature of 1300°C, and a sintering time of 1.5 hours. After cooling to room temperature, low-temperature sintered zirconia is obtained.
[0052] Example 4
[0053] The embodiment of the present invention provides a low-temperature sintered zirconia, which is prepared from the following raw materials in weight proportion: 84% zirconia powder, 8% rare earth oxide, 5% calcium carbonate, 1.5% polyvinyl alcohol, and 1.5% silicon dioxide.
[0054] The sintering temperature of the low-temperature sintered zirconia is 1400° C., and the sintering time is 1 hour.
[0055] In this embodiment, the low temperature sintered zirconia further includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0056] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol and silicon dioxide and continue mixing;
[0057] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 4 hours;
[0058] Step 3: The ball-milled powder is subjected to low-temperature sintering, with a heating rate of 5°C / min, a sintering temperature of 1400°C, and a sintering time of 1 hour. After cooling to room temperature, low-temperature sintered zirconia is obtained.
[0059] Example 5
[0060] The embodiment of the present invention provides a low-temperature sintered zirconia, which is prepared from the following raw materials in weight proportion: 85% of zirconia powder, 8% of rare earth oxide, 5% of calcium carbonate, 1% of polyvinyl alcohol, and 1% of silicon dioxide.
[0061] In this embodiment, the rare earth oxides are lanthanum oxide, gadolinium oxide, and yttrium oxide. The rare earth oxides are also doped with metal oxides, and the metal oxide is zirconium oxide. The content of the metal oxide is 0.1-1.0 wt%.
[0062] The sintering temperature of the low-temperature sintered zirconia is 1300° C., and the sintering time is 2 hours.
[0063] In this embodiment, the low temperature sintered zirconia further includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia is as follows:
[0064] Step 1: Mix zirconium oxide powder and rare earth oxide evenly, and add a set amount of calcium carbonate, polyvinyl alcohol, and silicon dioxide to continue mixing, wherein the additive is a rare earth oxide composed of lanthanum oxide, gadolinium oxide, and yttrium oxide;
[0065] Step 2: ball milling the mixed powder in air or oxygen atmosphere for 4 hours;
[0066] Step 3: The ball-milled powder is subjected to low-temperature sintering, with a heating rate of 5°C / min, a sintering temperature of 1300°C, and a sintering time of 2 hours. After cooling to room temperature, low-temperature sintered zirconia is obtained.
[0067] The performance of the low-temperature sintered zirconia prepared in Example 1 of the present invention was tested. The following tests were performed on the prepared low-temperature sintered zirconia: particle size analysis, specific surface area test, sintering performance test, and microstructure analysis.
[0068] The low-temperature sintered zirconia prepared in Example 1 is used to prepare dentures. The specific preparation method is to add the ball-milled powder into a mold, press it, then sinter it, and finally polish it to obtain high-quality dentures. The sintering temperature in the denture preparation process is 1200-1400°C, and the sintering time is 1-2 hours.
[0069] Testing denture performance: The prepared dentures were subjected to the following tests: hardness test, bending strength test, fracture toughness test, and microstructure analysis.
[0070] (1) Performance test data of low temperature sintered zirconia prepared in Example 1 are as follows in Table 1:
[0071] Table 1 Particle size analysis results
[0072] Particle size (μm) Volume fraction (%) 0.2~0.5 20 0.5~1.0 40 1.0~2.0 30
[0073] (2) Specific surface area test data: 10m 2 / g or so.
[0074] (3) Sintering performance test data: Sintering density: 6.0g / cm 3 , sintering shrinkage: 20%.
[0075] (4) Microstructure analysis data: The grain size is about 0.5 μm, with no obvious defects.
[0076] Test results:
[0077] The performance test results of the denture prepared by low temperature sintering zirconia in Example 1 are as follows:
[0078] Hardness test data: 1200HV;
[0079] Bending strength test data: 1200MPa;
[0080] Fracture toughness test data: 5MPa·m 1 / 2 ;
[0081] Microstructure analysis data: The denture tissue is dense and has no obvious defects.
[0082] In addition, the performance test results of the low temperature sintered zirconia prepared in Example 1 are as follows:
[0083] (1) Particle size analysis: The average particle size of the powder is about 0.5 μm, and the particle size distribution is uniform.
[0084] (2) Specific surface area test: Specific surface area is 10m 2 / g, indicating that the powder is relatively fine.
[0085] (3) Sintering performance test: sintering density is 6.0g / cm 3 The sintering shrinkage is about 20%.
[0086] (4) Microstructure analysis: The powder grains are small and uniform, with no obvious defects.
[0087] The performance test results of the denture prepared by low temperature sintering zirconia in Example 1 are as follows:
[0088] (1) Hardness test: The hardness of denture is 1200HV, which is relatively high.
[0089] (2) Bending strength test: The bending strength of the denture is 1200MPa, which is high.
[0090] (3) Fracture toughness test: The fracture toughness of the denture is 5 MPa·m 1 / 2 , with good toughness.
[0091] (4) Microstructural analysis: The denture tissue is dense and has no obvious defects.
[0092] From the above, it can be seen that the prepared low-temperature sintered zirconia has the advantages of uniform particle size distribution, fine grains, no obvious defects, and good sintering performance. The prepared denture has high hardness, high bending strength, good fracture toughness, good structural density and no obvious defects.
[0093] In summary, the low-temperature sintered zirconia provided by the present invention and its application in denture preparation have good performance and can be used in the field of oral restoration.
[0094] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.
Claims
1. A low temperature sintered zirconia, characterized in that: The low-temperature sintered zirconia is prepared from the following raw materials in proportion by weight: Zirconium oxide powder 84-90%, rare earth oxide 3-8%, calcium carbonate 2-5%, polyvinyl alcohol 0.5-1.5%, silicon dioxide 0.5-1.5%.
2. The low temperature sintered zirconia according to claim 1, characterized in that: The low-temperature sintered zirconium oxide is prepared from the following raw materials according to weight proportion: 88% zirconium oxide powder, 6% rare earth oxide, 4% calcium carbonate, 1% polyvinyl alcohol, and 1% silicon dioxide.
3. The low temperature sintered zirconia according to claim 1 or 2, characterized in that: The rare earth oxides are lanthanum oxide, gadolinium oxide and yttrium oxide.
4. The low temperature sintered zirconia according to claim 3, characterized in that: The rare earth oxide is further doped with a metal oxide, which is one of zirconium oxide, silicon nitride, aluminum nitride, titanium oxide, aluminum oxide, magnesium oxide and sodium oxide, and the content of the metal oxide is 0.1-1.0 wt%.
5. The low temperature sintered zirconia according to claim 1 or 2, characterized in that: The low temperature sintered zirconia also includes the preparation of the low temperature sintered zirconia. The preparation method of the low temperature sintered zirconia has the following steps: 1) mixing zirconium oxide powder and rare earth oxide uniformly, adding a set amount of calcium carbonate, polyvinyl alcohol, and silicon dioxide and continuing to mix, wherein the additive is a rare earth oxide composed of lanthanum oxide, gadolinium oxide, and yttrium oxide; 2) ball milling the mixed powder in air or oxygen atmosphere for 2-4 hours; 3) The ball-milled powder is subjected to low-temperature sintering at a sintering temperature of 1200-1400° C. for 1-2 hours to obtain low-temperature sintered zirconia.
6. The low temperature sintered zirconia according to claim 5, characterized in that: In an oxygen atmosphere, the heating rate is 5°C / min, the sintering temperature is 1200°C, and the temperature is kept for 1 hour, and then the temperature is cooled to room temperature to obtain low-temperature sintered zirconia.
7. The low temperature sintered zirconia according to claim 5, characterized in that: The density of the low-temperature sintered zirconia is greater than 98%, the strength of the low-temperature sintered zirconia is greater than 800MPa, and the thermal expansion coefficient of the low-temperature sintered zirconia is lower than 8×10^-6 / K.
8. The method for preparing low temperature sintered zirconia according to claim 5, characterized in that: The light transmittance of the low-temperature sintered zirconia is greater than 40%, and the polishability of the low-temperature sintered zirconia is less than Ra0.02μm.
9. A denture made of low temperature sintered zirconia according to any one of claims 5 to 8, characterized in that: In the preparation process of dentures, the sintering temperature is 1200-1400°C and the sintering time is 1-2 hours.
10. The denture made of low temperature sintered zirconia according to claim 9, characterized in that: The preparation method of the denture prepared by warm sintering zirconia is: adding the ball-milled powder into a mold, pressing, then sintering, and finally polishing to obtain the denture.
Citation Information
Patent Citations
Preparation method of zirconia ceramic false teeth
CN106388959A
Colored zirconia ceramic
CN107244914A
Zirconia sintered body and production method thereof
CN112624761A
Preparation method of high-performance gradient denture capable of realizing sintering consistency
CN117731432A
Dental orthodontic bracket and its production
JP1996033650A