Novel degradable nano dispersant as well as preparation method and application thereof
By combining halogenated spiropyran and polymethylallyl bispolyoxyethylene ether to form a new degradable dispersant of nanoparticles, the problem of sedimentation and flocculation of pesticide dispersants after use is solved, and stable dispersion and environmental protection are achieved. Friendly degradation, reducing environmental pollution.
Patent Information
- Application Number
- CN202410827581.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing pesticide dispersants are prone to sedimentation and flocculation after use, and the dispersants themselves may be prone to water absorption and excessive viscosity, resulting in unstable dispersion effects and difficulty in degrading in the environment, causing environmental pollution.
Using a new type of degradable nanodispersant, halogenated spiropyran and polymethylallyl bispolyoxyethylene ether are connected through ether bonds to form nanoparticles. The pesticide particles are stably dispersed through π-π bonds and electrostatic repulsion, and It is degraded into small molecules by sunlight and microbial action under natural conditions.
It achieves stable dispersion and environmentally friendly degradation of pesticide particles, reduces environmental pollution caused by polymer accumulation, improves the life and dispersion performance of the dispersant, and at the same time reduces the water absorption and viscosity of the dispersant.
Smart Images

Figure BDA0004910956980000021 
Figure BDA0004910956980000031 
Figure BDA0004910956980000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of dispersants, and specifically relates to a novel degradable nano dispersant and a preparation method and application thereof. Background Art
[0002] Dispersants can be roughly divided into anionic, cationic and nonionic types. They are mainly used to reduce the force of solid mixing into liquid. At present, dispersants have been widely used in paints, molding compositions, coatings, plastic compositions, printing inks, synthetic resins, pesticides and other systems. Pesticide preparations such as herbicides, insecticides, fungicides, etc. are generally prepared into wettable powders, water-dispersible granules, and suspensions, and their formulas generally contain dispersants. Although traditional dispersants such as alkylbenzene sulfonates, alkylphenol polyoxyethylene ethers, naphthalene sulfonate formaldehyde condensates, lignin sulfonates, etc. have certain dispersing and stabilizing effects, due to low molecular weight, unreasonable distribution of functional groups, poor environmental compatibility, etc., the dispersion effect of the obtained pesticide water suspension system is unstable and prone to sedimentation and flocculation.
[0003] In view of the above problems, the art mostly adopts the method of matching dispersant adjuvants or modifying existing dispersants to solve them. Patent CN107410300A discloses a polymer that can be used as a pesticide dispersant, which is copolymerized by glycidyl ether-terminated methyl allyl alcohol polyoxyethylene ether, methyl allyl alcohol polyoxyethylene ether ammonium sulfate, methacrylate, and methacrylic acid, and has good adsorption and dispersion effect, which is conducive to the preparation of a suspension system with stable performance; Patent CN109757471A discloses a pesticide dispersant, which is composed of a polycarboxylic acid dispersant, a polyether-modified polysiloxane, ethyl acetate, benzenesulfonic acid, CMC and water. The pesticide dispersant is non-toxic and harmless, has low sensitivity to pH value and temperature, reduces the viscosity of the dispersion system, has high dispersion stability, and is not prone to sedimentation and flocculation; Existing pesticide dispersants are mostly polymers. Although they improve the dispersibility and stability of the system to a certain extent, the dispersant itself may have the problem of easy water absorption and excessive viscosity, and cannot be weighed accurately, so it must be used with some additives.
[0004] Therefore, there is an urgent need in the market to prepare a new type of degradable nano-dispersant with good adsorption and dispersion effect and stable performance of the suspension system. Summary of the invention
[0005] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides a novel degradable nano-dispersant and a preparation method thereof. The novel degradable nano-dispersant obtained by the present invention can stably disperse pesticide particles, and after being used, can be degraded into small molecules under natural conditions, reducing environmental problems caused by the accumulation of macromolecules, and can be applied to pesticides.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is:
[0007] The first aspect of the present invention provides a novel degradable nano-dispersant, the structural formula of which is as follows:
[0008]
[0009] Among them, n, x, and y are all integers, 3≤n≤9, 50≤x≤55, 50≤y≤55.
[0010] The second aspect of the present invention provides a method for preparing a novel degradable nano-dispersant, comprising the following steps:
[0011] A1. Under the protection of inert gas, dissolve halogenated spiropyran, poly(methylallyl bisoxyethylene ether) and 4-dimethylaminopyridine in dichloromethane, stir at 25-35° C. for 35-37 hours, extract with dichloromethane, and combine and collect the organic phases;
[0012] A2, drying the organic phase obtained in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant;
[0013] A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 70-80° C. and 90-100 r / min, then put it into a hot press mold, and hot press at 110-120° C. and 16-18 MPa for 6-8 min to obtain the novel degradable nano-dispersant.
[0014] In the present invention, the dispersant is prepared as nanoparticles. Since the nanoparticles have a small particle size, they can be more easily adsorbed on the surface of the dispersed substance, thereby improving the dispersibility and wettability of the dispersed substance and forming a stable dispersion system.
[0015] In some embodiments, the molar ratio of halogenated spiropyran to poly(methyl allyl bis(oxyethylene) ether) in step A1 is (2-2.5):1.
[0016] Preferably, in step A1, the molar ratio of halogenated spiropyran to poly(methyl allyl bisoxyethylene ether) is 2.2:1.
[0017] The invention limits the molar ratio of halogenated spiropyran and polymethallyl bis-polyoxyethylene ether, thereby increasing the grafting rate of polymethallyl bis-polyoxyethylene ether, promoting the reaction to proceed in the forward direction, and accelerating the reaction rate.
[0018] In some embodiments, the halogenated spiropyran has the following structural formula:
[0019]
[0020] Wherein R is one of Cl and Br.
[0021] In some embodiments, the method for preparing the halogenated spiropyran comprises the following steps:
[0022] B1, dissolve 2,3,3-trimethyl-3H-indole and 2-bromoethanol in acetonitrile, heat under reflux at 75-85°C for 11-13h under an inert gas atmosphere, cool to 25-35°C, rotary evaporate, and wash with acetone to obtain solid-1;
[0023] B2, dissolving the solid-1 obtained in step B1 and 5-nitrosalicylicylaldehyde in ethanol, heating to reflux at 55-65°C, adding an ethanol solution of diethylamine, and continuing to heat to reflux for 4-6 hours under an inert gas atmosphere, rotary evaporation, washing, and purification by silica gel column chromatography to obtain solid-2;
[0024] B3. Add the solid-2 obtained in step B2 to N,N-dimethylformamide, add the halogenated sulfoxide while stirring, react at 0-5° C. for 3-5 hours, distill the product, collect the separated fractions, and obtain the halogenated spiropyran.
[0025] In some embodiments, the sulfoxide halide is one of sulfoxide chloride and sulfoxide bromide.
[0026] Preferably, the sulfoxide halide is thionyl chloride.
[0027] In some embodiments, the molar ratio of solid-2 to sulfoxide halide in step B3 is 1:(0.5-0.7).
[0028] Preferably, in step B3, the molar ratio of solid-2 to sulfoxide halide is 1:0.6.
[0029] The invention first prepares hydroxy spiropyran, further halogenates the hydroxyl group to obtain halogenated spiropyran, converts the hydroxyl group into halogen atoms so that it is easier to connect with the terminal hydroxyl group of polymethylallyl bis-polyoxyethylene ether, and the polymethylallyl bis-polyoxyethylene ether is connected with the spiropyran through an ether bond. Under the irradiation of visible light, the spiropyran is in a hydrophobic closed-loop state, so that the prepared nano-dispersant reduces water absorption and agglomeration, and the nano-particles are more uniform. When used, the ultraviolet light irradiates the ring to open the ring to a hydrophilic state, and the benzene ring on the spiropyran molecule can form a π-π bond with the molecular plane of the pesticide particle, and the two are firmly combined together. In addition, the steric hindrance and electrostatic repulsion of the polyoxyethylene ether bond make the pesticide particles stably dispersed. At the same time, the change of the structural spatial position during the ring opening further increases the dispersing ability of the dispersant. At the same time, the spiropyran also has certain antioxidant performance, slows down the breakage of the ether bond in the dispersant, and increases the life of the dispersant. After the dispersant is used, it can be degraded into small molecules through sunlight irradiation and microbial action in the natural environment, so as to prevent the accumulation of polymers from causing environmental pollution.
[0030] In some embodiments, the structural formula of the poly(meth)allyl bis(oxyethylene) ether is:
[0031]
[0032] Among them, n, x, and y are all integers, 3≤n≤9, 50≤x≤55, 50≤y≤55.
[0033] In some embodiments, the method for preparing the poly(meth)allyl bis(oxyethylene) ether comprises the following steps:
[0034] C1, dissolving methyl allyl polyoxyethylene ether in ethanol, stirring at 65-75° C. for 3-5 min under an inert gas atmosphere, adding an initiator, heating under reflux, controlling the weight average molecular weight to 4800-5000, adding a terminator, and obtaining a precipitated copolymer;
[0035] C2, washing the precipitated copolymer obtained in step C1, and drying at 30-35° C. for 8-10 hours to obtain the polymethylallyl bis(oxyethylene) ether.
[0036] The present invention polymerizes the carbon-carbon double bonds of methallyl bispolyoxyethylene ether and connects free methallyl polyoxyethylene ethers together to prepare polymethallyl bispolyoxyethylene ether, which is evenly distributed on the entire molecular chain. The pesticide is more easily adsorbed by the dispersant, and the molecular weight of the polymethallyl bispolyoxyethylene ether is further limited, so that the polymerization degree between the carbon-carbon double bonds is prevented from being too high, the chain length of the generated dispersant is too long, and the adsorption capacity of the alkyl chain on solid particles is too strong, resulting in the weakening of the steric hindrance of the polyoxyethylene ether, so that the dispersed substances are agglomerated.
[0037] The third aspect of the present invention provides an application of a novel degradable nano-dispersant in pesticides, wherein the dispersant accounts for 3-5 wt % in the pesticides.
[0038] Compared with the prior art, the present invention has the following beneficial effects:
[0039] 1. The present invention prepares a novel degradable nano-dispersant by using poly(methylallyl bis(oxyethylene) ether) and grafting spiropyran at its end, so that the pesticide particles can be stably dispersed. After use, the pesticide particles can be degraded into small molecules under natural conditions, thus reducing the environmental problems caused by the accumulation of high molecules.
[0040] 2. In the present invention, polymethyl allyl bis(oxyethylene) ether is connected to spiropyran through an ether bond. The benzene ring on the spiropyran molecule can form a π-π bond with the molecular plane of the pesticide particle. The two are firmly combined together, and the steric hindrance and electrostatic repulsion of the polyoxyethylene ether bond make the pesticide particles stably dispersed. At the same time, spiropyran also has certain antioxidant properties, which slows down the breakage of the ether bond in the dispersant and increases the life of the dispersant.
[0041] 3. In the present invention, the dispersant is prepared as nanoparticles. The nanoparticles have a small particle size and can be more easily adsorbed on the surface of the dispersed substance, thereby improving the dispersibility and wettability of the dispersed substance and forming a stable dispersion system. In addition, due to the closed-loop hydrophobicity of the spiropyran molecules, it is not easy to agglomerate during the preparation and storage process. When used, ultraviolet light irradiation opens the ring to a hydrophilic state, making the system evenly dispersed. At the same time, the change in the spatial position of the structure during the ring opening further increases the dispersing ability of the dispersant. DETAILED DESCRIPTION
[0042] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0043] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows:
[0044] Methyl allyl polyoxyethylene ether was purchased from Jingzhou Yinjie Chemical Co., Ltd., model: HPEG-2400.
[0045] Preparation Example 1
[0046] The preparation method of halogenated spiropyran-1 comprises the following steps:
[0047] B1, 3.18 g of 2,3,3-trimethyl-3H-indole and 2.54 g of 2-bromoethanol were dissolved in 25 g of anhydrous acetonitrile, heated to reflux at 80°C for 12 h under a nitrogen atmosphere, cooled to 30°C, rotary evaporated, and washed with acetone to obtain solid-1;
[0048] B2, 4.54g of solid-1 obtained in step B1 and 2.76g of 5-nitrosalicylicaldehyde were dissolved in 50g of anhydrous ethanol, heated to reflux at 60°C, and 15ml of anhydrous ethanol solution containing 3.6g of diethylamine was added. Under a nitrogen atmosphere, the mixture was heated to reflux for 5h, evaporated, washed with acetone, and purified by silica gel column chromatography to obtain solid-2;
[0049] B3. Add 5 g of solid-2 obtained in step B2 to 20 g of N,N-dimethylformamide, add 1.5 g of thionyl chloride while stirring, react at 2° C. for 4 h, distill the product, collect the separated fractions, and obtain the halogenated spiropyran-1.
[0050] Preparation Example 2
[0051] The preparation method of halogenated spiropyran-2 comprises the following steps:
[0052] B1, 3.18 g of 2,3,3-trimethyl-3H-indole and 2.54 g of 2-bromoethanol were dissolved in 25 g of anhydrous acetonitrile, heated to reflux at 80°C for 12 h under a nitrogen atmosphere, cooled to 30°C, rotary evaporated, and washed with acetone to obtain solid-1;
[0053] B2, 4.54g of solid-1 obtained in step B1 and 2.76g of 5-nitrosalicylicylaldehyde were dissolved in 50g of anhydrous ethanol, heated to reflux at 60°C, and 15ml of anhydrous ethanol solution containing 3.6g of diethylamine was added. Under a nitrogen atmosphere, the mixture was heated to reflux for 5h, and then rotary evaporated, washed, and purified by silica gel column chromatography to obtain solid-2;
[0054] B3. Add 5 g of solid-2 obtained in step B2 to 20 g of N,N-dimethylformamide, add 0.5 g of thionyl chloride while stirring, react at 2° C. for 4 h, distill the product, collect the separated fractions, and obtain the halogenated spiropyran-2.
[0055] Preparation Example 3
[0056] The preparation method of polymethallyl bisoxyethylene ether-1 comprises the following steps:
[0057] C1, dissolving 22g of methyl allyl polyoxyethylene ether in 100g of anhydrous ethanol, stirring at 70°C for 5min under a nitrogen atmosphere, adding 3.6g of benzoyl peroxide, heating under reflux, controlling the weight average molecular weight to 4885, adding 0.2g of hydroquinone, and obtaining a precipitated copolymer;
[0058] C2. Wash the precipitated copolymer obtained in step C1 with 500 ml of anhydrous ethanol for 3 times and dry at 35° C. for 10 h to obtain the poly(methyl allyl bisoxyethylene ether)-1, the structural formula of which is as follows:
[0059]
[0060] Among them, n=5, x=53, y=53.
[0061] Preparation Example 4
[0062] The preparation method of polymethallyl bisoxyethylene ether-2 comprises the following steps:
[0063] C1, dissolving 22g of methyl allyl polyoxyethylene ether in 100g of anhydrous ethanol, stirring at 70°C for 5min under a nitrogen atmosphere, adding 3.6g of benzoyl peroxide, heating under reflux, controlling the weight average molecular weight to 5546, adding 0.2g of hydroquinone, and obtaining a precipitated copolymer;
[0064] C2, washing the precipitated copolymer obtained in step C1 with 500 ml of anhydrous ethanol for 3 times, and drying at 35° C. for 10 h to obtain the poly(methyl allyl bisoxyethylene ether)-2, the structural formula of which is as follows:
[0065]
[0066] Among them, n=11, x=58, y=58.
[0067] Example 1
[0068] A novel degradable nano-dispersant, the structural formula of which is as follows:
[0069]
[0070] Among them, n=5, x=53, y=53.
[0071] The preparation method of the novel degradable nano-dispersant of this embodiment comprises the following steps:
[0072] A1. Under nitrogen protection, 6.8 g of halogenated spiropyran-1, 43.2 g of polymethylallyl bis(oxyethylene ether)-1 and 1.2 g of 4-dimethylaminopyridine were dissolved in 150 g of dichloromethane, stirred at 30 ° C for 36 h, then extracted with dichloromethane, and the organic phases were combined and collected;
[0073] A2, drying the organic phase in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant;
[0074] A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 75° C. and 95 r / min, then put it into a hot press mold, and hot press at 115° C. and 17 MPa for 7 min to obtain the novel degradable nano-dispersant.
[0075] Example 2
[0076] A novel degradable nano-dispersant, the structural formula of which is as follows:
[0077]
[0078] Among them, n=5, x=53, y=53.
[0079] The preparation method of the novel degradable nano-dispersant of this embodiment comprises the following steps:
[0080] A1. Under nitrogen protection, 6.8 g of halogenated spiropyran-1, 43.2 g of polymethylallyl bis(oxyethylene ether)-1 and 1.2 g of 4-dimethylaminopyridine were dissolved in 150 g of dichloromethane, stirred at 25 °C for 35 h, then extracted with dichloromethane, and the organic phases were combined and collected;
[0081] A2, drying the organic phase in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant;
[0082] A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 70° C. and 90 r / min, then put it into a hot press mold, and hot press at 110° C. and 16 MPa for 6 min to obtain the novel degradable nano-dispersant.
[0083] Example 3
[0084] A novel degradable nano-dispersant, the structural formula of which is as follows:
[0085]
[0086] Among them, n=5, x=53, y=53.
[0087] The preparation method of the novel degradable nano-dispersant of this embodiment comprises the following steps:
[0088] A1. Under nitrogen protection, 6.8 g of halogenated spiropyran-1, 43.2 g of polymethylallyl bis(oxyethylene ether)-1 and 1.2 g of 4-dimethylaminopyridine were dissolved in 150 g of dichloromethane, stirred at 35 ° C for 37 h, then extracted with dichloromethane, and the organic phases were combined and collected;
[0089] A2, drying the organic phase in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant;
[0090] A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 80° C. and 100 r / min, then put it into a hot press mold, and hot press at 120° C. and 18 MPa for 8 min to obtain the novel degradable nano-dispersant.
[0091] Example 4
[0092] This embodiment provides a novel biodegradable nanodispersant and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that the amount of halogenated spiropyran-1 added in step A1 is 3.4 g.
[0093] Example 5
[0094] This embodiment provides a novel biodegradable nanodispersant and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that in step A1, an equal amount of poly(meth)allyl bis(oxyethylene ether)-1 is replaced by poly(meth)allyl bis(oxyethylene ether)-2.
[0095] Example 6
[0096] This embodiment provides a novel degradable nanodispersant and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that in step A1, an equal amount of halogenated spiropyran-1 is replaced by halogenated spiropyran-2.
[0097] Comparative Example 1
[0098] A new type of degradable nanodispersant, the structural formula is as follows:
[0099]
[0100] The preparation method of the novel degradable nano-dispersant of this comparative example comprises the following steps:
[0101] A1. Under nitrogen protection, 6.8 g of halogenated spiropyran-1, 43.2 g of methyl allyl polyoxyethylene ether and 1.2 g of 4-dimethylaminopyridine were dissolved in 150 g of dichloromethane, stirred at 30 ° C for 36 h, then extracted with dichloromethane, and the organic phases were combined and collected;
[0102] A2, drying the organic phase in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant;
[0103] A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 75° C. and 95 r / min, then put it into a hot press mold, and hot press at 115° C. and 17 MPa for 7 min to obtain the novel degradable nano-dispersant.
[0104] Performance Testing:
[0105] 5 g of fluazinam and 0.2 g of the novel degradable nanodispersant prepared in each example and comparative example were added into 15 g of deionized water, irradiated under ultraviolet light for 2 h while stirring, and placed in a light-proof container as a test sample for later use.
[0106] 1. Determination of Suspension Rate
[0107] Determined according to "GB / T14825-2006 Method for Determination of Pesticide Suspension Rate".
[0108] 2. Persistent foaming test
[0109] Determined according to “GB / T28137-2011 Determination Method for Persistent Foaming of Pesticides”.
[0110] 3. Degradability test
[0111] Take the soil at a depth of 5 cm in the test field where the new degradable nano-dispersant obtained in the embodiments and comparative examples was used, and the weight-average molecular weight was tested. The test was conducted 10 times in parallel, and the average value was taken as m0. After 20 days, the soil sample at the same place was tested for the weight-average molecular weight, and the test was conducted 10 times in parallel, and the average value was taken as m1. The degradation rate was obtained, and the degradation rate = (m0-m1) / m0×100%.
[0112] The test results are shown in Table 1.
[0113] Table 1
[0114]
[0115] By comparing Examples 1-3 in the experimental data of Table 1, it can be seen that the new degradable nano-dispersant obtained by the present invention has good dispersibility and degradability; and the change in the ratio of poly(meth)allyl bis(oxyethylene) ether may lead to a decrease in the purity of the dispersant and a decrease in dispersibility; by comparing Example 1 and Example 4, it can be seen that the amount of halogenated spiropyran-1 added is changed, and the suspension rate decreases; by comparing Example 1 and Example 5, it can be seen that poly(meth)allyl bis(oxyethylene) ether-1 is replaced by poly(meth)allyl bis(oxyethylene) ether-2 in equal amounts, and the suspension rate and degradability are both reduced; by comparing Example 1 and Example 6, it can be seen that halogenated spiropyran-1 is replaced by halogenated spiropyran-2 in equal amounts, and the dispersibility and degradation rate are both reduced; by comparing Example 1 and Comparative Example 1, it can be seen that the suspension rate effect of the dispersant prepared using methallyl polyoxyethylene ether decreases.
[0116] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A novel degradable nanodispersant, characterized in that: The structural formula of the dispersant is as follows: Among them, n, x, and y are all integers, 3≤n≤9, 50≤x≤55, 50≤y≤55.
2. A method for preparing the novel degradable nanodispersant according to claim 1, characterized in that: The following steps are involved: A1. Under the protection of inert gas, dissolve halogenated spiropyran, poly(methylallyl bisoxyethylene ether) and 4-dimethylaminopyridine in dichloromethane, stir at 25-35° C. for 35-37 hours, extract with dichloromethane, and combine and collect the organic phases; A2, drying the organic phase obtained in step A1, filtering, and removing the solvent by distillation under reduced pressure to obtain a crude product, and purifying the crude product by silica gel column chromatography to obtain a degradable dispersant; A3. Add the degradable dispersant obtained in step A2 into a single screw extruder at an extrusion temperature of 70-80° C. and 90-100 r / min, then put it into a hot press mold, and hot press at 110-120° C. and 16-18 MPa for 6-8 min to obtain the novel degradable nano-dispersant.
3. The method for preparing the novel degradable nano-dispersant according to claim 2, characterized in that: In the step A1, the molar ratio of halogenated spiropyran to poly(methylallyl bis(oxyethylene) ether) is (2-2.5):
1.
4. The method for preparing the novel degradable nano-dispersant according to claim 2, characterized in that: The structural formula of the halogenated spiropyran is as follows: Wherein R is one of Cl and Br.
5. The method for preparing the novel degradable nano-dispersant according to claim 4, characterized in that: The preparation method of the halogenated spiropyran comprises the following steps: B1, dissolve 2,3,3-trimethyl-3H-indole and 2-bromoethanol in acetonitrile, heat under reflux at 75-85°C for 11-13h under an inert gas atmosphere, cool to 25-35°C, rotary evaporate, and wash with acetone to obtain solid-1; B2, dissolving the solid-1 obtained in step B1 and 5-nitrosalicylicylaldehyde in ethanol, heating to reflux at 55-65°C, adding an ethanol solution of diethylamine, and continuing to heat to reflux for 4-6 hours under an inert gas atmosphere, rotary evaporation, washing, and purification by silica gel column chromatography to obtain solid-2; B3. Add the solid-2 obtained in step B2 to N,N-dimethylformamide, add the halogenated sulfoxide while stirring, react at 0-5° C. for 3-5 hours, distill the product, collect the separated fractions, and obtain the halogenated spiropyran.
6. The method for preparing the novel degradable nano-dispersant according to claim 5, characterized in that: The sulfoxide halide is one of sulfoxide chloride and sulfoxide bromide.
7. The method for preparing the novel degradable nano-dispersant according to claim 5, characterized in that: The molar ratio of solid-2 to sulfoxide halide in step B3 is 1:(0.5-0.7).
8. The method for preparing the novel degradable nano-dispersant according to claim 2, characterized in that: The structural formula of the polymethylallyl bis(ethylene oxide) ether is: Among them, n, x, and y are all integers, 3≤n≤9, 50≤x≤55, 50≤y≤55.
9. The method for preparing the novel degradable nano-dispersant according to claim 8, characterized in that: The preparation method of the polymethylallyl bis(oxyethylene) ether comprises the following steps: C1. Dissolve methyl allyl polyoxyethylene ether in ethanol, stir at 65-75° C. for 3-5 min under an inert gas atmosphere, add an initiator, heat under reflux, control the molecular weight to 4800-5000, add a terminator, and obtain a precipitated copolymer; C2, washing the precipitated copolymer obtained in step C1, and drying at 30-35° C. for 8-10 hours to obtain the polymethylallyl bis(oxyethylene) ether.
10. Use of the novel degradable nano-dispersant according to claim 1 or the novel degradable nano-dispersant obtained by the preparation method according to any one of claims 2 to 9 in pesticides, characterized in that: The dispersant accounts for 3-5 wt % in the pesticide.
Citation Information
Cited By
Viscosity-reduced C80-grade concrete and preparation method thereof
CN119797859A