Epoxy resin material as well as preparation method and application thereof

Through the combination of bifunctional naphthyl epoxy resin and amine curing agent and multi-stage curing reaction, the problem of high-temperature curing and reactivity adjustment of epoxy resin materials is solved, and epoxy with high glass transition temperature and mechanical properties is realized. Resin material suitable for a variety of applications.

CN118755052APending Publication Date: 2024-10-11EAST CHINA UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411051950.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The need for existing epoxy resin materials to be cured at high temperatures limits their use in temperature-sensitive components, and it is difficult to adjust the reactivity to meet the needs of different application fields.

Method used

A combination of a bifunctional naphthyl epoxy resin matrix and an amine curing agent is used to prepare an epoxy resin material with adjustable reactivity by adjusting the epoxy value and the molar ratio of the amine curing agent, combined with appropriate mixing and removal. Bubble treatment, multi-stage curing reaction to obtain high glass transition temperature and excellent mechanical properties.

Benefits of technology

The reactivity of the epoxy resin material is adjustable, has high glass transition temperature and mechanical properties, simplifies the processing process, and is suitable for the fields of electronic packaging and composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755052A_ABST
    Figure CN118755052A_ABST
Patent Text Reader

Abstract

The invention discloses an epoxy resin material as well as a preparation method and application thereof. The raw material composition of the epoxy resin material comprises a bifunctional naphthyl epoxy resin matrix and an amine curing agent, wherein the amine curing agent is prepared from any one or two of m-phenylenediamine, diaminodiphenylmethane, 4, 4 '-diaminodiphenyl sulfone and isophorone diamine; wherein the epoxy value of the bifunctional naphthyl epoxy resin matrix is 0.65 mol / 100g to 0.73 mol / 100g; wherein the molar ratio of epoxy groups in the bifunctional naphthyl epoxy resin matrix to reactive hydrogen in the amine curing agent is 1: (0.8-1.2). The reaction activity of the epoxy resin material provided by the invention can be adjusted, and meanwhile, the epoxy resin material also has good mechanical strength and high glass transition temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an epoxy resin material and a preparation method and application thereof. Background Art

[0002] Epoxy resin generally refers to a high molecular weight oligomer that contains two or more epoxy groups in the molecular structure of the compound, with aliphatic, alicyclic or aromatic organic compounds as the basic molecular skeleton, and can form a three-dimensional cross-linked network thermosetting product through epoxy groups and other curing agents. Epoxy resin materials have excellent solvent resistance, heat resistance, electrical insulation, corrosion resistance and mechanical properties, so they are often used in adhesives, coatings, electronic packaging, automobiles, ships, and aerospace.

[0003] In the field of electronic packaging, epoxy resin is used as a packaging material for many optical devices such as LEDs and CMOS sensors, as well as electronic components such as chips. It provides the required physical and mechanical protection for the devices and has good transparency and electrical properties. However, many high-performance epoxy resin systems require long-term curing at high temperatures, which limits their use in devices with temperature-sensitive components. From the perspective of energy saving and large-scale production efficiency, this high-temperature curing condition is a disadvantage that cannot be ignored.

[0004] In the aerospace field, carbon fiber reinforced epoxy resin-based composite materials are used to make space shuttle doors, robotic arms and pressure vessels. Fiber winding is a composite molding process with high processing efficiency and good molding effect. Its product performance is uniform and stable. It is also the earliest developed and widely used technology. Among them, the dry winding molding process refers to the molding process in which the prepreg yarn is heated and softened to a viscous flow state on a winding machine and then wound onto a core mold. It has the advantages of environmental protection, easy use and high winding efficiency, but requires the resin matrix used to have low reactivity, high curing temperature, and moderate viscosity.

[0005] In addition, in order to ensure that the cured epoxy resin material can be used at a higher temperature, high requirements are placed on the material's glass transition temperature (Tg), dimensional stability, and mechanical properties. However, how to achieve that the reaction activity of the epoxy resin material can be adjusted according to the needs of the application field while having multiple requirements such as a high glass transition temperature and excellent mechanical strength is a technical problem that needs to be urgently solved in this field. Summary of the invention

[0006] The present invention mainly provides an epoxy resin material and a preparation method and application thereof to overcome the defect of the epoxy resin material in the prior art that its reaction activity affects subsequent processing. The epoxy resin material provided by the present invention can adjust its reaction activity and also has good mechanical strength and high glass transition temperature.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions.

[0008] In a first aspect, the present invention provides a raw material composition of an epoxy resin material, which comprises: a bifunctional naphthyl epoxy resin matrix and an amine curing agent;

[0009] Wherein, the amine curing agent includes any one or two of m-phenylenediamine, diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone and isophoronediamine;

[0010] Wherein, the epoxy value of the bifunctional naphthyl epoxy resin matrix is ​​0.65-0.73 mol / 100g;

[0011] Wherein, the molar ratio of the epoxy groups in the bifunctional naphthyl epoxy resin matrix to the active hydrogen in the amine curing agent is 1:(0.8-1.2).

[0012] In the present invention, the bifunctional naphthyl epoxy resin matrix may have the meaning commonly understood in the art, and generally refers to an epoxy resin matrix containing two epoxy groups and naphthyl groups in the molecular structure.

[0013] The epoxy group may be conventional in the art, generally referring to an ethylene oxide group.

[0014] In the present invention, the difunctional naphthyl epoxy resin matrix is ​​preferably 2,2'-[1,6-naphthylenebis(oxymethylene)]dioxirane, 2,2'-[1,5-naphthylenebis(oxymethylene)]dioxirane, 2,2'-[2,7-naphthylenebis(oxymethylene)]dioxirane, and more preferably 2,2'-[1,6-naphthylenebis(oxymethylene)]dioxirane.

[0015] In some specific embodiments, the difunctional naphthyl epoxy resin matrix may have a market grade of EBA-65.

[0016] In the present invention, the epoxy value of the difunctional naphthyl epoxy resin matrix generally refers to the amount of epoxy groups contained in 100 g of the difunctional naphthyl epoxy resin.

[0017] In the present invention, the epoxy value of the bifunctional naphthyl epoxy resin matrix may be 0.65-0.70 mol / 100g.

[0018] In some specific embodiments, the epoxy value of the difunctional naphthyl epoxy resin matrix is ​​0.66 mol / 100 g, 0.68 mol / 100 g, 0.69 mol / 100 g, or 0.72 mol / 100 g.

[0019] In the present invention, the molar ratio of the epoxy groups in the bifunctional naphthyl epoxy resin matrix to the active hydrogen in the amine curing agent is preferably 1:(0.85-1.2), such as 1:0.85, 1:0.875, 1:0.9, 1:1, 1:1.125 or 1:1.2.

[0020] In the present invention, the viscosity of the bifunctional naphthyl epoxy resin matrix at 50±1° C. may be 1500-2000 mPa·s, such as 1500 mPa·s, 1600 mPa·s, 1800 mPa·s, 1900 mPa·s or 2000 mPa·s.

[0021] In some specific embodiments, the viscosity of the difunctional naphthyl epoxy resin matrix at 50±1° C. can be 1826 mPa·s, 1857 mPa·s, 1833 mPa·s, 1990 mPa·s or 1960 mPa·s.

[0022] In the present invention, the active hydrogen of the amine curing agent generally refers to the active hydrogen on the nitrogen atom in its molecular structure.

[0023] In the present invention, the amount of the amine curing agent can be 15-60 parts by weight, preferably 16-55 parts by weight.

[0024] In the present invention, the mass ratio of the bifunctional naphthyl epoxy resin matrix to the amine curing agent can be 100:(16-55), for example, 100:16.276, 100:18.6, 100:37.45, 100:42.8, 100:51.36 or 100:54.5, in parts by weight.

[0025] In some specific embodiments, the raw material composition of the epoxy resin material includes, by weight: 100 parts of EBA-65 and 18.6 parts of m-phenylenediamine, and the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the m-phenylenediamine is 1:1.

[0026] In some specific embodiments, the raw material composition of the epoxy resin material includes, by weight, 100 parts of EBA-65, 13.02 parts of m-phenylenediamine and 8.79 parts of isophoronediamine, and the molar ratio of the epoxy group of the EBA-65, the active hydrogen of the m-phenylenediamine and the active hydrogen of the isophoronediamine is 1:0.7:0.3.

[0027] In some specific embodiments, the raw material composition of the epoxy resin material includes, by weight: 100 parts of EBA-65 and 34.2 parts of diaminodiphenylmethane, and the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the diaminodiphenylmethane is 1:1.

[0028] In some specific embodiments, the raw material composition of the epoxy resin material includes, by weight: 100 parts of EBA-65 and 37.45 parts of 4,4'-diaminodiphenyl sulfone, and the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the 4,4'-diaminodiphenyl sulfone is 1:0.875.

[0029] In some specific embodiments, the raw material composition of the epoxy resin material includes, by weight, 100 parts of EBA-65, 34.24 parts of 4,4'-diaminodiphenyl sulfone and 6.84 parts of diaminodiphenylmethane, and the molar ratio of the epoxy group of the EBA-65, the active hydrogen of the 4,4'-diaminodiphenyl sulfone and the active hydrogen of the diaminodiphenylmethane is 1:0.8:0.2.

[0030] In a second aspect, the present invention provides a method for preparing an epoxy resin material, which comprises the following steps: subjecting the raw material composition of the epoxy resin material as described above to a curing reaction to obtain the epoxy resin material.

[0031] In the present invention, before the curing reaction, the raw material composition is preferably mixed and defoamed in sequence.

[0032] The mixing method may be conventional in the art, generally stirring.

[0033] The mixing time is preferably 1-2.5 h, such as 1 h, 1.2 h, 1.5 h or 2 h.

[0034] The mixing temperature is preferably 25-125°C, such as 25°C, 27°C, 53°C, 55°C, 60°C, 115°C or 120°C.

[0035] The defoaming temperature is preferably 25-115°C, such as 25°C, 50°C, 53°C, 55°C, 108°C or 110°C.

[0036] The defoaming time is preferably 5 min-120 min, for example 5 min, 10 min, 15 min, 20 min, 40 min, 50 min, 60 min, 90 min or 120 min.

[0037] In the present invention, the temperature of the curing reaction may be 70-250°C.

[0038] In the present invention, the curing reaction time may be 8-13 hours.

[0039] In some specific embodiments, the curing reaction can be divided into four stages, namely, the first stage, the second stage, the third stage and the fourth stage;

[0040] The temperature of the first stage is preferably 140-150°C, such as 140°C, 145°C or 150°C; the duration of the first stage is preferably 2-3h, such as 2h, 2.5h or 3h.

[0041] The temperature of the second stage is preferably 155-190°C, such as 155°C, 160°C or 190°C; the duration of the second stage is preferably 2-3h, such as 2h, 2.5h or 3h.

[0042] The temperature of the third stage is preferably 190-230° C., such as 190° C., 220° C. or 230° C.; the duration of the third stage is preferably 2-3 h, such as 2 h, 2.5 h or 3 h.

[0043] The temperature of the fourth stage is preferably 230-250°C, such as 230°C, 235°C or 250°C; the duration of the fourth stage is preferably 1.5-2.5h, such as 1.5h, 2h or 2.5h.

[0044] In some specific embodiments, the curing reaction can be divided into two stages, namely a first stage and a second stage.

[0045] The temperature of the first stage is preferably 60-80°C, such as 60°C, 70°C or 80°C; the duration of the second stage is preferably 1-5h, such as 2h, 4h or 5h.

[0046] The temperature of the second stage is preferably 90-110°C, such as 90°C, 100°C or 110°C; the duration of the second stage is preferably 2-7h, such as 2h, 5h or 6h.

[0047] In a third aspect, the present invention provides an epoxy resin material, which is prepared by the preparation method as described above.

[0048] In a fourth aspect, the present invention provides the use of the epoxy resin material as described above in the field of electronic packaging or the field of composite materials.

[0049] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0050] The reagents and raw materials used in the present invention are commercially available.

[0051] The positive and progressive effects of the present invention are:

[0052] The present invention realizes the provision of epoxy resin materials with different reaction activities according to different application fields by using a bifunctional naphthyl epoxy resin matrix and controlling the epoxy value thereof to be 0.65-0.73 mol / 100 g, one or two amine curing agents, and the coordination between the molar ratio of the epoxy group and the active hydrogen in the amine curing agent, and at the same time has a high glass transition temperature and better mechanical properties, thereby achieving the goal of easy processing and high performance of the epoxy resin material. BRIEF DESCRIPTION OF THE DRAWINGS

[0053] Figure 1 The DSC curve of the resin solution forming a homogeneous system through step (1) in Example 1-5.

[0054] Figure 2 The DSC curve of the resin solution in comparative example 1-6 formed into a homogeneous system through step (1).

[0055] Figure 3 1 is the tensile (stress-strain) curve of the epoxy resin material specimens in Examples 1-5.

[0056] Figure 4 It is the tensile (stress-strain) curve of the epoxy resin material specimen in Comparative Examples 1-6.

[0057] Figure 5 The DSC curve of the resin solid formed in step (3) in Example 1-5.

[0058] Figure 6 The DSC curve of the resin solid formed in step (3) in Comparative Examples 1-6. DETAILED DESCRIPTION

[0059] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0060] The epoxy resin matrix EBA-65 used in the following Examples 1-5 and Comparative Examples 1, 5, and 6 is a bifunctional naphthyl-containing epoxy resin purchased from Shanghai Huayi Resin Co., Ltd., and its parameters are as follows:

[0061] Viscosity (50±1℃): 1500-2000mPa·s

[0062] Epoxy value: 0.65-0.73mol / 100g

[0063] Non-volatile matter: ≥98.5%

[0064] Epoxy value Viscosity at 50±1℃ Example 1 0.68mol / 100g 1826mPa·s Example 2 0.72mol / 100g 1857mPa·s Example 3 0.69mol / 100g 1833mPa·s Example 4 0.72mol / 100g 1990mPa·s Example 5 0.69mol / 100g 1960mPa·s

[0065] The epoxy resin matrix AG-80 used in Comparative Example 2 is a tetrafunctional epoxy resin purchased from Shanghai Huayi Resin Co., Ltd., and its parameters are as follows:

[0066] Viscosity (50±1℃): 3500mPa·s

[0067] Epoxy value: 0.85mol / 100g

[0068] Non-volatile matter: ≥98.5%

[0069] The epoxy resin matrix AFG90-MH used in Comparative Example 3 is a trifunctional epoxy resin purchased from Shanghai Huayi Resin Co., Ltd., and its parameters are as follows:

[0070] Viscosity (25±1℃): 2500mPa·s

[0071] Epoxy value: 1.01mol / 100g

[0072] Non-volatile matter: ≥99.5%

[0073] The epoxy resin matrix E51 used in Comparative Example 4 is a bifunctional liquid epoxy resin purchased from Shanghai Titan Technology Co., Ltd., and its parameters are as follows:

[0074] Viscosity (40±1℃): 2250mPa·s

[0075] Epoxy value: 0.51mol / 100g

[0076] Non-volatile matter: ≥98%

[0077] Example 1

[0078] (1) Mixing:

[0079] Weigh 100g of brand EBA-65 epoxy resin matrix and 18.6g of m-phenylenediamine, and add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture, in which the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:1; stir the above mixture at a constant temperature of 53°C for 1h until the solid amine curing agent is dissolved, then evacuate the flask and stir at 53°C under vacuum for 25min until all the amine curing agents are completely dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0080] (2) Defoaming:

[0081] The above resin solution was poured into a stainless steel mold preheated at 50°C, and then the mold was placed in a 50°C vacuum oven for 50 minutes to remove bubbles in the resin solution.

[0082] (3) Curing:

[0083] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction was divided into two stages, wherein the temperature of the first stage was 70°C and the duration of the first stage was 4 hours; the temperature of the second stage was 100°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a reddish-brown epoxy resin material was obtained.

[0084] Example 2

[0085] (1) Mixing

[0086] Weigh 100g of EBA-65 epoxy resin matrix and 13.02g of m-phenylenediamine, add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture, in which the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:0.7; first stir the above mixture at a constant temperature of 55°C for 1h until the solid amine curing agent is dissolved, then evacuate the flask and stir it at 55°C under vacuum for 20min. Then, let the above mixture pass through the atmosphere for 20min to cool to 25°C, add 8.79g of isophorone diamine, in which the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:0.7:0.3, and stir it under vacuum for 10min until all the amine curing agents are completely dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0087] (2) Defoaming

[0088] The above resin solution was poured into a stainless steel mold, and then the mold was placed in a vacuum oven at 30° C. for 15 min to remove bubbles in the resin solution.

[0089] (3) Curing

[0090] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction was divided into two stages, wherein the temperature of the first stage was 70°C and the duration of the first stage was 4 hours; the temperature of the second stage was 100°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a reddish-brown epoxy resin material was obtained.

[0091] Example 3

[0092] (1) Mixing

[0093] Weigh 100g of EBA-65 epoxy resin matrix and 34.2g of diaminodiphenylmethane. Add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:1. Stir the above mixture at a constant temperature of 56°C for 1.2h until the solid is dissolved, then evacuate the flask and stir at 56°C under vacuum for 30min until all the solids are dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0094] (2) Defoaming

[0095] The above resin solution was poured into a stainless steel mold preheated at 60°C, and then the mold was placed in a 60°C vacuum oven for 40 minutes to remove bubbles in the resin solution.

[0096] (3) Curing

[0097] The stainless steel mold containing the resin solution was then placed in an oven for curing. The curing reaction included four stages, wherein the temperature of the first stage was 70°C and the duration of the first stage was 4 hours; the temperature of the second stage was 100°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a reddish-brown specimen of epoxy resin material was obtained.

[0098] Example 4

[0099] (1) Mixing

[0100] Weigh 100 g of the epoxy resin matrix of the above-mentioned brand EBA-65 and 37.45 g of 4,4'-diaminodiphenyl sulfone, and add the above components respectively into a single-mouth round-bottom flask with a vacuum port to obtain a mixture, in which the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:0.875; stir the above mixture at a constant temperature of 115° C. for 40 minutes until the solid amine curing agent is dissolved, then evacuate the flask and stir at a vacuum state of 110° C. for 30 minutes until all the amine curing agents are completely dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0101] (2) Defoaming

[0102] The above resin solution was poured into a stainless steel mold preheated at 110°C, and then the mold was placed in a vacuum oven at 110°C for 90 minutes to remove bubbles in the resin solution.

[0103] (3) Curing step:

[0104] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction was divided into four stages, wherein the temperature of the first stage was 150°C and the duration of the first stage was 3 hours; the temperature of the second stage was 190°C and the duration of the second stage was 2.5 hours; the temperature of the third stage was 220°C and the duration of the third stage was 2 hours; the temperature of the fourth stage was 250°C and the duration of the fourth stage was 2 hours. After the resin solution was naturally cooled to room temperature, a dark red-brown epoxy resin material was obtained.

[0105] Example 5

[0106] (1) Weigh 100 g of the epoxy resin matrix of the above-mentioned brand EBA-65 and 34.24 g of 4,4'-diaminodiphenyl sulfone; add the above components respectively into a single-mouth round-bottom flask with a vacuum port to obtain a mixture, first stir the above mixture at a constant temperature of 115° C. for 40 minutes until the solid amine curing agent is dissolved, then evacuate the flask, stir it at 110° C. under vacuum for 30 minutes, then open the above mixture to the atmosphere, add 6.84 g of diaminodiphenylmethane, in which the molar ratio of the epoxy group of EBA-65, the active hydrogen of m-phenylenediamine and the active hydrogen of diaminodiphenylmethane is 1:0.8:0.2, and stir it under vacuum for 20 minutes until all the amine curing agent is completely dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0107] (2) Defoaming

[0108] The above resin solution was poured into a stainless steel mold preheated at 108°C, and then the mold was placed in a vacuum oven at 108°C for 40 minutes to remove bubbles in the resin solution.

[0109] (3) Curing

[0110] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction was divided into four stages, wherein the temperature of the first stage was 140°C and the duration of the first stage was 2 hours; the temperature of the second stage was 160°C and the duration of the second stage was 2 hours; the temperature of the third stage was 190°C and the duration of the third stage was 3 hours; the temperature of the fourth stage was 230°C and the duration of the fourth stage was 2 hours. After the resin solution was naturally cooled to room temperature, a dark red-brown epoxy resin material was obtained.

[0111] Comparative Example 1

[0112] (1) Mixing

[0113] Weigh 100g of the epoxy resin matrix of the above-mentioned brand EBA-65, 100g of methyltetrahydrophthalic anhydride and 0.5g of 2-ethyl-4-methylimidazole, and add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture, in which the molar ratio of the epoxy group of EBA-65 to the anhydride group of the anhydride curing agent is 1:0.87. Stir the above mixture at a constant temperature of 55°C for 50min until the solid is dissolved, then evacuate the flask and stir it at 55°C under vacuum for 30min until all the solid is dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0114] (2) Defoaming

[0115] The above resin solution was poured into a stainless steel mold preheated at 60°C, and then the mold was placed in a 60°C vacuum oven for 40 minutes to remove bubbles in the resin solution.

[0116] (3) Curing step:

[0117] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction includes four stages, wherein the temperature of the first stage is 120°C and the duration of the first stage is 2 hours; the temperature of the second stage is 135°C and the duration of the second stage is 4 hours; the temperature of the third stage is 150°C and the duration of the third stage is 3 hours; the temperature of the fourth stage is 170°C and the duration of the fourth stage is 2 hours. After the resin solution is naturally cooled to room temperature, a dark red-brown specimen of epoxy resin material is obtained.

[0118] Comparative Example 2

[0119] (1) Mixing

[0120] Weigh 100g of the epoxy resin matrix of the above-mentioned brand AG-80, 129g of methyl nadic anhydride and 1.5g of 2-ethyl-4-methylimidazole. Add the above components respectively into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of AG-80 to the anhydride group of the methyl nadic anhydride curing agent is 1:0.85. Stir the above mixture at a constant temperature of 55°C for 1h until the solid is dissolved, then evacuate the flask and stir at 55°C under vacuum for 40min until all the solids are dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0121] (2) Defoaming

[0122] The above resin solution was poured into a stainless steel mold preheated at 60°C, and then the mold was placed in a 60°C vacuum oven for 40 minutes to remove bubbles in the resin solution.

[0123] (3) Curing

[0124] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing reaction includes four stages, wherein the temperature of the first stage is 125°C and the duration of the first stage is 2 hours; the temperature of the second stage is 140°C and the duration of the second stage is 4 hours; the temperature of the third stage is 155°C and the duration of the third stage is 3 hours; the temperature of the fourth stage is 165°C and the duration of the fourth stage is 2 hours. After the resin solution is naturally cooled to room temperature, a black sample of epoxy resin material is obtained.

[0125] Comparative Example 3

[0126] (1) Mixing

[0127] Weigh 100g of the epoxy resin matrix of the above-mentioned brand AFG-90MH and 44.6g of diethyltoluenediamine. Add the above components separately into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of AFG-90MH to the active hydrogen of the amine curing agent is 1:1. Stir the above mixture at 37°C for 1h until the liquid is evenly mixed, then evacuate the flask and stir it under vacuum at 37°C for 30min until no obvious bubbles are seen in the flask.

[0128] (2) Defoaming

[0129] The above resin solution was poured into a stainless steel mold preheated at 60°C, and then the mold was placed in a 60°C vacuum oven for 40 minutes to remove bubbles in the resin solution.

[0130] (3) Curing

[0131] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing method was a two-step method. During the curing process, the temperature of the first stage was 130°C and the duration of the first stage was 4 hours; the temperature of the second stage was 180°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a dark yellow sample of epoxy resin material was obtained.

[0132] Comparative Example 4

[0133] (1) Mixing

[0134] Weigh 100g of E51 epoxy resin matrix and 31.67g of 4,4'-diaminodiphenyl sulfone. Add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of E51 to the active hydrogen of the amine curing agent is 1:1. Stir the above mixture at a constant temperature of 120℃ for 1h until the solid is dissolved, then evacuate the flask and stir at 115℃ under vacuum for 45min until all the solids are dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0135] (2) Defoaming

[0136] The above resin solution was poured into a stainless steel mold preheated at 110°C, and then the mold was placed in a vacuum oven at 110°C for 45 minutes to remove bubbles in the resin solution.

[0137] (3) Curing

[0138] Then, the stainless steel mold containing the resin solution is placed in an oven for curing. The curing reaction includes four stages, wherein the temperature of the first stage is 150°C and the duration of the first stage is 3 hours; the temperature of the second stage is 180°C and the duration of the second stage is 3 hours; the temperature of the third stage is 210°C and the duration of the third stage is 3 hours; the temperature of the fourth stage is 240°C and the duration of the fourth stage is 3 hours. After the resin solution is naturally cooled to room temperature, a white transparent sample of epoxy resin material is obtained.

[0139] Comparative Example 5

[0140] Preparation of epoxy resin material:

[0141] (1) Mixing step:

[0142] Weigh 100g of EBA-65 epoxy resin matrix and 24.18g of m-phenylenediamine. Add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:1.3. Stir the above mixture at a constant temperature of 53°C for 1h until the solid amine curing agent dissolves, then evacuate the flask and stir at 53°C under vacuum for 25min until all the amine curing agents are dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0143] (2) Defoaming

[0144] The above resin solution was poured into a stainless steel mold preheated at 50°C, and then the mold was placed in a 50°C vacuum oven for 50 minutes to remove bubbles in the resin solution.

[0145] (3) Curing

[0146] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing method was a two-step method. During the curing process, the temperature of the first stage was 70°C and the duration of the first stage was 4 hours; the temperature of the second stage was 100°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a reddish-brown epoxy resin material was obtained.

[0147] Comparative Example 6

[0148] (1) Mixing

[0149] Weigh 100g of EBA-65 epoxy resin matrix, 9.2g of diethyltoluenediamine, 5.58g of m-phenylenediamine, and 13.68g of diaminodiphenylmethane. Add the above components into a single-mouth round-bottom flask with a vacuum port to obtain a mixture. In the mixture, the molar ratio of the epoxy group of EBA-65 to the active hydrogen of the amine curing agent is 1:0.3:0.3:0.4. Stir the above mixture at a constant temperature of 53°C for 1h until the solid amine curing agent dissolves, then evacuate the flask and stir at 53°C under vacuum for 25min until all the amine curing agents are dissolved in the epoxy resin matrix to form a homogeneous system of the resin solution.

[0150] (2) Defoaming

[0151] The above resin solution was poured into a stainless steel mold preheated at 50°C, and then the mold was placed in a 50°C vacuum oven for 50 minutes to remove bubbles in the resin solution.

[0152] (3) Curing

[0153] Then, the stainless steel mold containing the resin solution was placed in an oven for curing. The curing method was a two-step method. During the curing process, the temperature of the first stage was 70°C and the duration of the first stage was 4 hours; the temperature of the second stage was 100°C and the duration of the second stage was 6 hours. After the resin solution was naturally cooled to room temperature, a reddish-brown epoxy resin material was obtained.

[0154] Effect Example

[0155] The present invention tests the curing temperature, mechanical properties and glass transition temperature of the epoxy resin materials in Examples 1-5 and Comparative Examples 1-6 by the following test methods:

[0156] (1) DSC test of curing temperature and glass transition temperature of epoxy resin material

[0157] The homogeneous resin solution system prepared in step (1) of Examples 1-5 and Comparative Examples 1-6 of the present invention was subjected to DSC test immediately after being uniformly mixed: in a nitrogen atmosphere, the temperature was raised from 25°C to 280°C at 5°C / min, and the curing temperature of the epoxy resin material was calculated by the temperature rise curve; the solid particles of the cured epoxy resin were heated to 250°C at 20°C / min, and the glass transition temperature of the epoxy resin material was calculated by the temperature rise curve. The determination of the curing temperature and the glass transition temperature was carried out in accordance with GB / T 19466.1-2004, and only integers were retained for temperature-related data.

[0158] (2) Epoxy resin material tensile properties test

[0159] The epoxy resin materials in Examples 1-5 and Comparative Examples 1-6 were prepared into dumbbell-shaped tensile specimens, and then the tensile properties were tested in accordance with GB / T 2567-2021.

[0160] Table 1 Curing start temperature, peak temperature and end temperature of epoxy resin materials obtained in Examples 1-5 and Comparative Examples 1-6

[0161]

[0162] Table 2 Mechanical properties of epoxy resin materials obtained in Examples 1-5 and Comparative Examples 1-6

[0163]

[0164]

[0165] The present invention provides epoxy resin materials with different activities and good mechanical properties suitable for different fields by adjusting the formula. Compared with various complicated epoxy resin categories on the market, the selection and trial and error costs are greatly saved.

[0166] Figure 1 The DSC curve of the resin solution formed into a homogeneous system through step (1) in Example 1-5. Figure 1 From the DSC curve of the resin solution forming a homogeneous system in step (1), it can be seen that the peak curing temperatures of Examples 1-3 are between 113°C and 122°C, and the peak curing temperatures of Examples 4 and 5 are between 190°C and 198°C.

[0167] Figure 2 The DSC curve of the resin solution formed into a homogeneous system by step (1) in Comparative Example 1-6. Figure 2 It can be seen that the peak curing temperature of Comparative Examples 1-6 is 124-218°C

[0168] Figure 3 is the tensile (stress-strain) curve of the epoxy resin material strip in Examples 1-5. Figure 3 It can be seen that the tensile strength of the epoxy resin material specimens of Examples 1-5 is 103.11-124.87 MPa, the tensile modulus is 3.30-4.04 GPa, and the elongation at break is 4.20-8.11%.

[0169] Figure 4 is the tensile (stress-strain) curve of the epoxy resin material strip in Comparative Examples 1-6. Figure 4It can be seen that the tensile strength of the epoxy resin material specimens of Comparative Examples 1-6 is 45.22-114.01 MPa, the tensile modulus is 3.18-4.03 GPa, and the elongation at break is 1.37-5.81%.

[0170] Figure 5 The DSC curve of the resin solid formed in step (3) of Example 1-5 shows that the glass transition temperature Tg corresponding to the midpoint of the step of the second heating curve of Example 1-5 is 180-225°C.

[0171] Figure 6 The DSC curve of the resin solid formed in step (3) in Comparative Examples 1-6 shows that the glass transition temperature Tg corresponding to the midpoint of the step of the second heating curve is 149-243°C.

[0172] Comparative Example 1 uses an anhydride curing agent, and Comparative Example 2 uses a tetrafunctional epoxy resin matrix. It can be seen from the data in Table 1 and Table 2 that Comparative Examples 1 and 2 have lower reaction activity, high curing temperature, low glass transition temperature and poor mechanical properties.

[0173] The functionality and epoxy value of the epoxy resin matrix of Comparative Examples 3 and 4 are not within the scope of the present invention. It can be seen from the data in Table 1 and Table 2 that Comparative Examples 3 and 4 have lower reactivity, high curing temperature, low glass transition temperature and poor mechanical properties.

[0174] The molar ratio of epoxy group to active hydrogen in Comparative Example 5 is not within the scope of the present invention. It can be seen from the data in Table 1 and Table 2 that Comparative Example 5 has a high curing temperature, a low glass transition temperature and poor mechanical properties.

[0175] In Comparative Example 6, three amine curing agents were used, which had no significant effect on improving the mechanical properties. Moreover, due to the complex composition of the three curing agents, the processing technology was more complicated than that of the present invention, and the activity was too high, which was not conducive to storage.

[0176] The embodiments described above are only some embodiments of the present invention, which are convenient for those skilled in the art to understand and use the present invention. Obviously, any person skilled in the art can slightly modify or change the present embodiment and apply it to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and any equal changes, simple modifications and modifications made within the scope of the present invention still belong to the scope of the present invention.

Claims

1. A raw material composition of epoxy resin material, characterized in that: It includes: bifunctional A naphthyl epoxy resin matrix and an amine curing agent; Wherein, the amine curing agent includes any one or two of m-phenylenediamine, diaminodiphenylmethane, 4,4'-diaminodiphenyl sulfone and isophoronediamine; Wherein, the epoxy value of the bifunctional naphthyl epoxy resin matrix is ​​0.65-0.73 mol / 100g; Wherein, the molar ratio of the epoxy groups in the bifunctional naphthyl epoxy resin matrix to the active hydrogen in the amine curing agent is 1:(0.8-1.2).

2. The raw material composition of the epoxy resin material according to claim 1, characterized in that The difunctional naphthyl epoxy resin matrix is ​​2,2'-[1,6-naphthylene di(oxymethylene)] dioxirane, 2,2'-[1,5-naphthylene di(oxymethylene)] dioxirane, 2,2'-[2,7-naphthylene di(oxymethylene)] dioxirane, preferably 2,2'-[1,6-naphthylene di(oxymethylene)] dioxirane; and / or, the epoxy value of the difunctional naphthyl epoxy resin matrix is ​​0.65-0.70 mol / 100 g, such as 0.66 mol / 100 g, 0.68 mol / 100 g or 0.69 mol / 100 g; And / or, the molar ratio of epoxy groups in the bifunctional naphthyl epoxy resin matrix to active hydrogen in the amine curing agent is 1:(0.85-1.2), for example, 1:0.85, 1:0.875, 1:0.9, 1:1, 1:1.125 or 1:1.

2.

3. The raw material composition of the epoxy resin material according to claim 1, characterized in that The bifunctional naphthyl epoxy resin matrix has a viscosity of 1500-2000 mPa·s at 50±1° C., such as 1500 mPa·s, 1600 mPa·s, 1800 mPa·s, 1900 mPa·s, 1826 mPa·s, 1857 mPa·s, 1833 mPa·s, 1990 mPa·s or 1960 mPa·s or 2000 mPa·s; And / or, in parts by weight, the amount of the amine curing agent is 15-60 parts, preferably 16-55 parts; And / or, in parts by weight, the mass ratio of the bifunctional naphthyl epoxy resin matrix to the amine curing agent is 100:(16-55), for example, 100:16.276, 100:18.6, 100:37.45, 100:42.8, 100:51.36 or 100:54.

5.

4. The raw material composition of the epoxy resin material according to claim 1, characterized in that The raw material composition of the epoxy resin material includes, by weight: 100 parts of EBA-65 and 18.6 parts of m-phenylenediamine, wherein the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the m-phenylenediamine is 1:1; Or, in parts by weight, the raw material composition of the epoxy resin material includes: 100 parts of EBA-65, 34.2 parts of diaminodiphenylmethane, and the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the diaminodiphenylmethane is 1:1 Or, in parts by weight, the raw material composition of the epoxy resin material comprises: 100 parts of EBA-65, 13.02 parts of m-phenylenediamine and 8.79 parts of isophoronediamine, and the molar ratio of the epoxy group of the EBA-65, the active hydrogen of the m-phenylenediamine and the active hydrogen of the isophoronediamine is 1:0.7:0.3; Or, in parts by weight, the raw material composition of the epoxy resin material comprises: 100 parts of EBA-65 and 37.45 parts of 4,4'-diaminodiphenyl sulfone, and the molar ratio of the epoxy group of the EBA-65 to the active hydrogen of the 4,4'-diaminodiphenyl sulfone is 1:0.875; Alternatively, the raw material composition of the epoxy resin material comprises, in parts by weight: 100 parts of EBA-65, 34.24 parts of 4,4'-diaminodiphenyl sulfone and 6.84 parts of diaminodiphenylmethane, and the molar ratio of the epoxy group of the EBA-65, the active hydrogen of the 4,4'-diaminodiphenyl sulfone and the active hydrogen of the diaminodiphenylmethane is 1:0.8:0.

2.

5. A method for preparing an epoxy resin material, characterized in that: The method comprises the following steps: subjecting the raw material composition of the epoxy resin material according to any one of claims 1 to 4 to a curing reaction to obtain the epoxy resin material.

6. The method for preparing the epoxy resin material according to claim 5, characterized in that: Before the curing reaction, the raw material composition is mixed and defoamed in sequence; Wherein, the mixing time is preferably 1-2.5h, such as 1h, 1.2h, 1.5h or 2h; Wherein, the mixing temperature is preferably 25-125°C, such as 25°C, 27°C, 53°C, 55°C, 60°C, 115°C or 120°C; Wherein, the defoaming temperature is preferably 25-115°C, such as 25°C, 50°C, 53°C, 55°C, 108°C or 110°C; The defoaming time is preferably 5 min-120 min, for example 5 min, 10 min, 15 min, 20 min, 40 min, 50 min, 60 min, 90 min or 120 min.

7. The method for preparing the epoxy resin material according to claim 5, characterized in that: The curing reaction temperature is 70-250°C; And / or, the curing reaction time is 8-13 hours.

8. The method for preparing the epoxy resin material according to claim 5, characterized in that: The curing reaction is divided into four stages, namely the first stage, the second stage, the third stage and the fourth stage; The temperature of the first stage is preferably 140-150°C, such as 140°C, 145°C or 150°C; the duration of the first stage is preferably 2-3h, such as 2h, 2.5h or 3h; The temperature of the second stage is preferably 155-190°C, such as 155°C, 160°C or 190°C; the duration of the second stage is preferably 2-3h, such as 2h, 2.5h or 3h; The temperature of the third stage is preferably 190-230°C, such as 190°C, 220°C or 230°C; the duration of the third stage is preferably 2-3h, such as 2h, 2.5h or 3h; The temperature of the fourth stage is preferably 230-250°C, such as 230°C, 235°C or 250°C; the duration of the fourth stage is preferably 1.5-2.5h, such as 1.5h, 2h or 2.5h; Or, the curing reaction is divided into two stages, namely a first stage and a second stage; The temperature of the first stage is preferably 60-80°C, such as 60°C, 70°C or 80°C; the duration of the second stage is preferably 1-5h, such as 2h, 4h or 5h; The temperature of the second stage is preferably 90-110°C, such as 90°C, 100°C or 110°C; the duration of the second stage is preferably 2-7h, such as 2h, 5h or 6h.

9. An epoxy resin material, characterized in that: It is prepared by the preparation method according to any one of claims 5 to 8.

10. Use of the epoxy resin material according to claim 9 in the field of electronic packaging or composite materials.

Citation Information

Patent Citations

  • Epoxy resin containing naphthalene ring structure and preparation method thereof

    CN113861383A

  • Crystalline 1,5-diglycidylnaphthalene and cured products thereof

    US3635843A