Preparation method of polyamide 66 with high strength and high elongation at break

By using specific comonomers and processing aids in the preparation of polyamide 66 resin, the problem that traditional polyamide 66 resin is difficult to maintain high strength and high elongation at break at the same time is solved, and the high strength of polyamide 66 resin is achieved. High elongation at break and notched impact strength improve its performance in engineering plastics and fiber products.

CN118755080APending Publication Date: 2024-10-11JIANGSU YANGNONG CHEMICAL GROUP CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411061736.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Traditional polyamide 66 resin is difficult to maintain high strength and high elongation at break at the same time, resulting in reduced impact resistance in low-temperature environments, limiting its application in engineering plastics and fiber products.

Method used

By using dibasic acid or diamine comonomers with a specific structure and adding processing aids during the preparation process of polyamide 66 resin, the synergistic effect is to increase the elongation at break and notched impact strength while maintaining high strength and High modulus properties.

Benefits of technology

Significantly improves the elongation at break and notched impact strength of polyamide 66 resin, improves its toughness and processability in engineering plastics and fiber products, while maintaining high strength and high modulus properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004979627490000191
    Figure BDA0004979627490000191
Patent Text Reader

Abstract

The invention relates to a preparation method of polyamide 66 with high strength and high elongation at break. The resin is prepared from the following raw materials: a) adipic acid; b) hexamethylenediamine; c) a comonomer; and d) a processing aid. The invention also relates to a method for preparing the resin. The method comprises the following steps: i) mixing adipic acid and hexamethylenediamine and dissolving in water; ii) adding a comonomer and a processing aid into the mixture obtained in the step i); iii) subjecting the mixture obtained in step ii) to polymerization. The present application further relates to a composition comprising said resin or a resin prepared by said method. Further, the present application relates to the use of the combination of the comonomer and the processing aid for improving the elongation at break and / or notch impact strength of the PA66 resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polyamide 66 polymerization, and in particular to a method for preparing a polyamide 66 resin which can maintain intrinsic high strength properties and has high elongation at break properties. Background Art

[0002] Polyamide 66 has high strength, good wear resistance, excellent fatigue resistance, good chemical corrosion resistance and self-lubricating properties. It can be widely used in engineering plastics, industrial yarns, textile and clothing fibers, and films. However, polyamide 66 has some shortcomings of its own: such as low elongation at break, which leads to brittle fracture, and greatly reduced impact resistance in low temperature environments, which seriously limits the application of polyamide 66. Elongation at break is one of the important indicators that determine the processing conditions of polyamide 66 and the performance of its products. Especially for fiber products, elongation at break is an important indicator to characterize the softness and elasticity of fibers. Fibers with large elongation at break feel softer and can dissipate the tensile stress during spinning, thereby reducing hair and broken ends; but the elongation at break should not be too large, otherwise the fabric will be easily deformed. The elongation at break of polyamide 66 resin is generally required to be between 15 and 40%. However, it is difficult for traditional polyamide 66 resin to balance the relationship between strength and elongation at break at the same time.

[0003] The reports on high elongation at break polyamide 66 resin and its preparation in the existing literature are as follows:

[0004] Patent CN 116554463 A mixes 10 to 90 parts by weight of nylon 66 salt, 10 to 90 parts by weight of caprolactam, and 0 to 5 parts by weight of aliphatic or aromatic diacid / diamine, and prepares a high-toughness copolyamide 6 / 66 by ternary copolymerization, which significantly improves the elongation at break and notched impact strength. However, the strength and modulus of the copolyamide are greatly reduced by about 20%.

[0005] Patent CN 106832911 A reacts a DOPO-based reactive phosphorus flame retardant with a diamine to obtain a flame retardant salt, which is then added to a 66 salt polymerization system to obtain a flame retardant polyamide 66 resin with a high elongation at break. The polyamide molecular chain is composed of a polyamide 66 segment and a DOPO-based reactive phosphorus flame retardant segment, with an elongation at break of up to 30 to 60%. It can be injection molded into engineering plastic products such as gears and bearings, and can also be spun into polyamide 66 fibers, etc. However, the tensile strength of the polyamide resin is reduced to 60 to 74 MPa.

[0006] Patent CN 107513163 A adds a mixture obtained by reacting acrylate, amino-containing organic acid and organic base to a 66 salt solution, and polymerizes to obtain a high-toughness polyamide 66 resin. The elongation at break of the polyamide 66 resin is greater than 80%, and the notched impact strength is greater than 10KJ / m 2 , and exhibits excellent transparency. However, its tensile strength is reduced to 60 to 70 MPa.

[0007] The above-mentioned prior arts have effectively improved the elongation at break and notched impact performance of polyamide 66 resin, but inevitably weakened the strength and modulus of the material.

[0008] Therefore, a polyamide 66 preparation process is needed that can overcome the above-mentioned problems in the prior art, so that the obtained polyamide 66 resin not only maintains the characteristics of high strength and high modulus, but also overcomes the defect of easy brittle fracture of traditional polyamide 66 resin, and exhibits excellent elongation at break and impact resistance. Summary of the invention

[0009] One of the purposes of the present application is to provide a method for preparing high-strength and high-elongation-at-break polyamide 66 resin.

[0010] The first aspect of the present application provides a resin prepared from raw materials comprising:

[0011] a) adipic acid;

[0012] b) hexamethylenediamine;

[0013] c) comonomers;

[0014] d) processing aids,

[0015] wherein the comonomer is selected from the group consisting of C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines, with the proviso that the comonomer is different from adipic acid or hexamethylenediamine, and

[0016] The processing aid is selected from the group consisting of fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof.

[0017] The comonomer may be optionally substituted. For example, the comonomer may be optionally substituted by one or more of a C1 to C12 hydrocarbon group, a C1 to C12 alkoxy group, a C1 to C12 acyl group, a C3 to C12 aryl group, a C3 to C12 aralkyl group, a C3 to C12 alkaryl group, or a C3 to C12 heteroaryl group substituted by hydroxyl, halogen, amino, amine, or thiol.

[0018] The second aspect of the present application provides a method for preparing the resin described in the first aspect of the present application, the method comprising the following steps:

[0019] i) mixing adipic acid and hexamethylenediamine and dissolving them in water;

[0020] ii) adding comonomers and processing aids to the mixture obtained in step i);

[0021] iii) subjecting the mixture obtained in step ii) to polymerization;

[0022] wherein the comonomer is selected from the group consisting of C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines, with the proviso that the comonomer is different from adipic acid or hexamethylenediamine, and

[0023] The processing aid is selected from the group consisting of fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof.

[0024] The third aspect of the present application provides a composition comprising the resin described in the first aspect of the present application or a resin prepared by the method described in the second aspect of the present application.

[0025] The fourth aspect of the present application provides an article prepared from the resin described in the first aspect of the present application or the composition described in the third aspect of the present application.

[0026] The fifth aspect of the present application provides use of the combination of the comonomer and the processing aid as described above for improving the elongation at break of PA66 resin.

[0027] The sixth aspect of the present application provides the use of the combination of the comonomer and the processing aid as described above for improving the elongation at break of PA66 resin.

[0028] The applicant has unexpectedly found that the purpose of the present application can be achieved by adding a dibasic acid or diamine comonomer of a specific structure and a processing aid during the polymerization of polyamide 66. The comonomer and the processing aid produce a synergistic effect. The prepared polyamide 66 resin can not only maintain the intrinsic high-strength and high-modulus properties, but also significantly improve the elongation at break and the notched impact strength. This helps to improve the toughness of polyamide 66 plastic products, as well as the spinnability and flexibility of its fiber products. DETAILED DESCRIPTION

[0029] "Scope" disclosed herein is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be inclusive or exclusive of end values, and can be arbitrarily combined, i.e., any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following range can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0 to 5" means that all real numbers between "0 to 5" are listed in this document, and "0 to 5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0030] In this application, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.

[0031] In this application, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.

[0032] In the present application, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0033] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0034] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number itself, and "several" in "one or several" means two or more.

[0035] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0036] Herein, unless otherwise specified, percentage (%) or part refers to percentage by weight or part by weight relative to the composition.

[0037] Herein, if there is no contrary description, the sum of the contents of the various components in the composition is 100%.

[0038] Herein, if there is no contrary description, the sum of the parts of each component in the composition may be 100 parts by weight.

[0039] In this document, unless otherwise specified, "a combination thereof" means a multi-component mixture of the elements described, for example a mixture of two, three, four and up to the maximum possible multi-component mixture.

[0040] If not specifically stated, the terms "a" or "an" used in the present specification means "at least one".

[0041] Herein, unless otherwise stated, all reactions are carried out at normal temperature and pressure.

[0042] The first aspect of the present application provides a resin prepared from raw materials comprising:

[0043] a) adipic acid;

[0044] b) hexamethylenediamine;

[0045] c) comonomers;

[0046] d) processing aids,

[0047] wherein the comonomer is selected from the group consisting of C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines, with the proviso that the comonomer is different from adipic acid or hexamethylenediamine, and

[0048] The processing aid is selected from the group consisting of fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof.

[0049] The comonomer may be optionally substituted. For example, the comonomer may be optionally substituted with one or more of a C1 to C12 alkyl group, a C1 to C12 alkoxy group, a C1 to C12 acyl group, a C3 to C12 aryl group, a C3 to C12 aralkyl group, a C3 to C12 alkaryl group, or a C3 to C12 heteroaryl group substituted with a hydroxyl, a halogen, an amino, an amine, a thiol.

[0050] Comonomer

[0051] In the context of the present application, if not specifically stated otherwise, the terms "comonomer" and "third monomer" are used interchangeably and mean a monomer different from adipic acid or hexamethylenediamine but copolymerizable with adipic acid and hexamethylenediamine.

[0052] According to one embodiment, the comonomer is selected from C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines.

[0053] In one embodiment of the present application, the comonomer content is 0.001 to 2 wt%, or 0.001 to 1.8 wt%, or 0.001 to 1.6 wt%, or 0.001 to 1.4 wt%, or 0.001 to 1.2 wt%, or 0.001 to 1.0 wt%, or 0.001 to 0.8 wt%, or 0.001 to 0.6 wt%, or 0.001 to 0.4 wt%, or 0.001 to 0.2 wt%, relative to the total weight of component a) and component b). For example, the comonomer content can be 0.05 wt%, or 0.1 wt%, or 0.15 wt%, or 0.2 wt%, or 0.25 wt%, or 0.3 wt%, or 0.35 wt%, or 0.4 wt%, or 0.45 wt%, or 0.5 wt%, or 0.55 wt%, or 0.6 wt%, or 0.65 wt%, or 0.7 wt%, or 0.75 wt%, or 0.8 wt%, or 0.85 wt%, or 0.9 wt%, or 0.95 wt%, or 1.0 wt%, or 1.1 wt%. %. 0.05 wt. %, or 1.1 wt. %, or 1.15 wt. %, or 1.2 wt. %, or 1.25 wt. %, or 1.3 wt. %, or 1.35 wt. %, or 1.4 wt. %, or 1.45 wt. %, or 1.5 wt. %, or 1.55 wt. %, or 1.6 wt. %, or 1.65 wt. %, or 1.7 wt. %, or 1.75 wt. %, or 1.8 wt. %, or 1.85 wt. %, or 1.9 wt. %, or 1.95 wt. %, or 2 wt. %, relative to the total weight of component a) and component b).

[0054] In a preferred embodiment, the comonomer is selected from C3 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 aliphatic diacids, which may be optionally substituted with one or more of C1 to C12 hydrocarbon groups substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl.

[0055] According to a preferred embodiment, the comonomer is selected from the group consisting of malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, 2-methylmalonic acid, 2,2-dimethylmalonic acid, 2-methylsuccinic acid, 2-butylsuccinic acid, 2-cyclohexylsuccinic acid, 2-acetylsuccinic acid, 2-p-tolylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, phenylsuccinic acid, benzylsuccinic acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 2,4-diethylglutaric acid, 3,3-dimethylglutaric acid, 3,3-tetramethyleneglutaric acid, and 3-ethyl-3-methylglutaric acid.

[0056] In another preferred embodiment, the comonomer is selected from C4 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 alicyclic diacids, which may be optionally substituted with one or more of C1 to C12 hydrocarbon groups substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl.

[0057] According to a preferred embodiment, the comonomer is selected from: cyclopentanedicarboxylic acid, cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, cyclooctanedicarboxylic acid, cyclononanedicarboxylic acid, cyclodecanedicarboxylic acid, decahydronaphthalene dicarboxylic acid, 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, which may be optionally substituted by one or more of C1 to C12 hydrocarbon groups substituted by hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl.

[0058] In another preferred embodiment, the comonomer is selected from C3 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 aliphatic diamines.

[0059] In a preferred embodiment, the comonomer is selected from the group consisting of propylene diamine, butylene diamine, pentylene diamine, hexylene diamine, heptylene diamine, octanediamine, nonane diamine, decane diamine, undecane diamine, dodecane diamine, 2-methylpropylene diamine, 2,2-dimethylpropylene diamine, 2-methylbutylene diamine, 2-butylbutylene diamine, 2-cyclohexylbutylene diamine, 2-acetylbutylene diamine, 2-p-tolylbutylene diamine, 2,2-dimethylbutylene diamine, 2,3-dimethylbutylene diamine, phenylbutylene diamine, benzylbutylene diamine, 2-methylpentane diamine, 3-methylpentane diamine, 2,2-dimethylpentane diamine, 2,4-diethylpentane diamine, 3,3-dimethylpentane diamine, 3,3-tetramethylenepentane diamine, and 3-ethyl-3-methylpentane diamine.

[0060] In another preferred embodiment, the comonomer is selected from C4 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 cycloaliphatic diamines.

[0061] According to a preferred embodiment, the comonomer is selected from: cyclopentanediamine, cyclohexanediamine, cycloheptanediamine, cyclooctanediamine, cyclononanediamine, cyclodecanediamine, decahydronaphthalenediamine, isophoronediamine, 1,2,2-trimethyl-1,3-cyclopentanediamine, 1,3-cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, and 2-aminocyclopentylmethylamine.

[0062] Hexamethylenediamine and adipic acid

[0063] The molar number of component a) adipic acid and the molar number of component b) hexamethylenediamine in the raw material may be equal or unequal.

[0064] In one embodiment, the number of moles of adipic acid, component a), is greater than the number of moles of hexamethylenediamine, component b), for example, the molar ratio of component a) to component b) is 1 to 1.1, or 1 to 1.09, or 1 to 1.08, or 1 to 1.07, or 1 to 1.06, or 1 to 1.05, or 1 to 1.04, or 1 to 1.03, or 1 to 1.02, or 1 to 1.01, or 1 to 1.005, or 1 to 1.001, or 1 to 1.0005, or 1 to 1.0001.

[0065] In another embodiment, the number of moles of adipic acid, component a), is less than the number of moles of hexamethylenediamine, component b), for example, the molar ratio of component a) to component b) is from 0.9 to 1, or from 0.91 to 1, or from 0.92 to 1, or from 0.93 to 1, or from 0.94 to 1, or from 0.95 to 1, or from 0.96 to 1, or from 0.97 to 1, or from 0.98 to 1, or from 0.99 to 1, or from 0.995 to 1, or from 0.999 to 1, or from 0.9995 to 1, or from 0.9999 to 1.

[0066] Processing Aids

[0067] In the context of this application, the term "processing aid" means a component which can adjust the final properties of the product.

[0068] According to a non-limiting embodiment, the processing aid is selected from: fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof.

[0069] According to one embodiment, the fatty acids in the fatty acid esters, fatty acid salts and fatty acid amides are selected from C2 to C30 fatty acids, preferably C3 to C29 fatty acids, preferably C4 to C28 fatty acids, preferably C5 to C27 fatty acids, preferably C6 to C26 fatty acids, preferably C7 to C25 fatty acids, preferably C8 to C24 fatty acids, preferably C9 to C23 fatty acids, preferably C10 to C22 fatty acids, preferably C11 to C21 fatty acids, preferably C12 to C20 fatty acids, preferably C13 to C19 fatty acids, preferably C14 to C18 fatty acids, preferably C15 to C17 fatty acids, preferably C16 fatty acids.

[0070] As non-limiting examples, the fatty acid can be acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, heptanoic acid, caprylic acid, nonanoic acid, capric acid, lauric acid, myristic acid, palmitic acid, oleic acid, stearic acid, isostearic acid, behenic acid, montanic acid.

[0071] According to one embodiment, the fatty acid ester is an ester of a fatty acid with an alcohol of C2 to C30, preferably C3 to C29, preferably C4 to C28, preferably C5 to C27, preferably C6 to C26, preferably C7 to C25, preferably C8 to C24, preferably C9 to C23, preferably C10 to C22, preferably C11 to C21, preferably C12 to C20, preferably C13 to C19, preferably C14 to C18, preferably C15 to C17, preferably C16 fatty alcohol.

[0072] Preferably, the alcohol is an aliphatic monohydric alcohol, such as pentadecanol, cetyl alcohol, heptadecyl alcohol, stearyl alcohol, nonadecanol, eicosanol, wax alcohol, myricyl alcohol; an aliphatic polyhydric alcohol, such as 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, glycerol, pentaerythritol; an alicyclic diol, such as cyclopentane-1,2-diol, cyclohexane-1,2-diol, cyclohexane-1,4-diol.

[0073] For example, you can use

[0074] - aliphatic monocarboxylic acid esters such as cetyl laurate, benzoylmethyl laurate, cetyl myristate, benzoylmethyl myristate, isopropylidene palmitate, dodecyl palmitate, tetradecyl palmitate, pentadecyl palmitate, octadecyl palmitate, cetyl palmitate, phenyl palmitate, benzoylmethyl palmitate, cetyl stearate, ethyl behenate;

[0075] - Monoesters of ethylene glycol such as glycol monolaurate, glycol monopalmitate, and glycol monostearate; diesters of ethylene glycol such as glycol dilaurate, glycol dipalmitate, and glycol distearate;

[0076] - monoesters of glycerol, such as glyceryl monolaurate, glyceryl monomyristate, glyceryl monopalmitate, glyceryl monostearate;

[0077] - diesters of glycerol, such as glyceryl dilaurate, glyceryl dimyristate, glyceryl dipalmitate, glyceryl distearate;

[0078] - triesters of glycerol, such as trilaurin, trimyristin, tripalmitin, tristearin, dioleyl palmitate, distearyl palmitate, distearyl oleate;

[0079] - Esters of pentaerythritol, such as pentaerythritol tetrastearate.

[0080] According to one embodiment, the fatty acid salt is an alkali metal salt, an alkaline earth metal salt, an aluminum salt, or a transition metal salt of a fatty acid.

[0081] For example, the fatty acid salt may be selected from:

[0082] - acetates, such as sodium acetate, potassium acetate, magnesium acetate, calcium acetate;

[0083] - laurates, such as sodium laurate, potassium laurate, potassium hydrogen laurate, magnesium laurate, calcium laurate, zinc laurate, silver laurate;

[0084] - myristates, such as lithium myristate, sodium myristate, potassium hydrogen myristate, magnesium myristate, calcium myristate, zinc myristate, silver myristate;

[0085] - palmitates, such as lithium palmitate, potassium palmitate, magnesium palmitate, calcium palmitate, zinc palmitate, copper palmitate, lead palmitate, thallium palmitate, cobalt palmitate;

[0086] - oleates, such as sodium oleate, potassium oleate, magnesium oleate, calcium oleate, zinc oleate, lead oleate, thallium oleate, copper oleate, nickel oleate;

[0087] - stearates, such as sodium stearate, lithium stearate, magnesium stearate, calcium stearate, barium stearate, aluminum stearate, thallium stearate, lead stearate, nickel stearate, beryllium stearate;

[0088] - isostearates such as sodium isostearate, potassium isostearate, magnesium isostearate, calcium isostearate, barium isostearate, aluminum isostearate, zinc isostearate, nickel isostearate;

[0089] - behenate salts, such as sodium behenate, potassium behenate, magnesium behenate, calcium behenate, barium behenate, aluminum behenate, zinc behenate, nickel behenate;

[0090] - montanic acid salts, such as sodium montanate, potassium montanate, magnesium montanate, calcium montanate, barium montanate, aluminum montanate, zinc montanate, nickel montanate.

[0091] More preferably, the fatty acid salt is selected from stearates and montanates, and particularly preferably selected from sodium stearate, potassium stearate, zinc stearate, barium stearate, aluminum stearate, sodium montanate, and calcium montanate.

[0092] According to one embodiment, the fatty acid amide is selected from:

[0093] - aliphatic monocarboxylic acid amides, such as lauric acid amide, palmitic acid amide, oleic acid amide, stearic acid amide, erucic acid amide, behenic acid amide, ricinoleic acid amide, hydroxystearic acid amide;

[0094] - N-substituted aliphatic monocarboxylic acid amides, such as N-oleyl palmitamide, N-oleyl oleamide, N-oleyl stearamide, N-stearyl oleamide, N-stearyl stearamide, N-stearyl erucamide, hydroxymethyl stearamide, hydroxymethyl behenamide;

[0095] - aliphatic dicarboxylic acid amides, such as methylenebisstearamide, ethylenebislauric acid amide, ethylenebiscaproic acid amide, ethylenebisoleic acid amide, ethylenebisoleic acid amide, ethylenebisstearic acid amide, ethylenebiserucic acid amide, ethylenebisbehenic acid amide, ethylenebisisostearic acid amide, ethylenebishydroxystearic acid amide, butylenebisstearic acid amide, hexamethylenebisoleic acid amide, hexamethylenebisstearic acid amide, hexamethylenebisbehenic acid amide, hexamethylenebishydroxystearic acid amide, meta-xylylenebisstearic acid amide, meta-xylylenebis-12-hydroxystearic acid amide;

[0096] - N-substituted aliphatic carboxylic acid bisamides, such as N,N'-dioleyl sebacic acid amide, N,N'-dioleyl adipamide, N,N'-distearyl adipamide, N,N'-distearyl sebacic acid amide, N,N'-distearyl isophthalic acid amide, N,N'-distearyl terephthalic acid amide;

[0097] - N-substituted ureas such as N-butyl-N'-stearyl urea, N-propyl-N'-stearyl urea, N-stearyl-N'-stearyl urea, N-phenyl-N'-stearyl urea, benzyldimethyl distearyl urea, distilbenes distearyl urea, hexamethylene distearyl urea, diphenylmethane distearyl urea, diphenylmethane bislauryl urea.

[0098] As a preferred embodiment, the processing aid is selected from pentaerythritol stearate, ethylene bisoleamide, rice bran wax, aluminum stearate, calcium montanate, sodium montanate or a mixture thereof.

[0099] However, it should be understood that the processing aids that can be used in the present application are not limited thereto.

[0100] The amount of processing aid depends on the desired properties of the final product. In a non-limiting embodiment, the content of the processing aid can be 0.001 to 2 weight %, or 0.001 to 1.8 weight %, or 0.001 to 1.6 weight %, or 0.001 to 1.4 weight %, or 0.001 to 1.2 weight %, or 0.001 to 1.0 weight %, or 0.001 to 0.8 weight %, or 0.001 to 0.6 weight %, or 0.001 to 0.4 weight %, or 0.001 to 0.3 weight %, or 0.001 to 0.2 weight %, or 0.001 to 0.1 weight %, relative to the total weight of component a) and component b). For example, the content of the processing aid may be 0.05 wt%, or 0.1 wt%, or 0.15 wt%, or 0.2 wt%, or 0.25 wt%, or 0.3 wt%, or 0.35 wt%, or 0.4 wt%, or 0.45 wt%, or 0.5 wt%, or 0.55 wt%, or 0.6 wt%, or 0.65 wt%, or 0.7 wt%, or 0.75 wt%, or 0.8 wt%, or 0.85 wt%, or 0.9 wt%, or 0.95 wt%, or 1.0 wt%, or 1.1 wt%. %. 0.05 wt. %, or 1.1 wt. %, or 1.15 wt. %, or 1.2 wt. %, or 1.25 wt. %, or 1.3 wt. %, or 1.35 wt. %, or 1.4 wt. %, or 1.45 wt. %, or 1.5 wt. %, or 1.55 wt. %, or 1.6 wt. %, or 1.65 wt. %, or 1.7 wt. %, or 1.75 wt. %, or 1.8 wt. %, or 1.85 wt. %, or 1.9 wt. %, or 1.95 wt. %, or 2 wt. %, relative to the total weight of component a) and component b).

[0101] The applicant of the present application has unexpectedly discovered that the comonomer and the processing aid produce a synergistic effect, so that the toughness of the obtained polyamide resin is significantly improved (for example, the elongation at break and the notched impact strength are significantly improved), while at the same time the inherent high strength and high modulus properties of the PA66 resin are maintained.

[0102] Accelerator

[0103] According to a preferred embodiment, the resin described in the first aspect of the present application further comprises component e) an accelerator.

[0104] In the context of this application, the term "accelerator" means any species that is capable of increasing the rate of a polymerization reaction.

[0105] As a non-limiting example, the accelerator may be selected from hypophosphites. According to a preferred embodiment, the accelerator is manganese hypophosphite or magnesium hypophosphite.

[0106] The amount of the accelerator depends on the desired properties of the final product. In a non-limiting example, the content of the accelerator can be 0 to 0.1% by weight, relative to the total weight of component a) adipic acid and component b) hexamethylenediamine in the raw material. For example, the content of the accelerator can be 1 to 500 ppm by weight, or 1 to 450 ppm by weight, or 1 to 400 ppm by weight, or 1 to 350 ppm by weight, or 1 to 300 ppm by weight, or 1 to 250 ppm by weight, or 1 to 200 ppm by weight, or 1 to 150 ppm by weight, or 1 to 100 ppm by weight, or 1 to 80 ppm by weight, or 1 to 60 ppm by weight, or 1 to 40 ppm by weight, or 1 to 20 ppm by weight, relative to the total weight of component a) and component b).

[0107] Thermal antioxidant

[0108] According to a preferred embodiment, the raw material of the resin in the first aspect of the present application further includes component f) a thermal oxidation inhibitor.

[0109] The thermal oxidation inhibitor may be any species that can inhibit thermal oxidation degradation and thus improve the thermal stability of the polyamide 66 resin.

[0110] According to a preferred embodiment, the thermal oxidant can be one or more of copper salt, cuprous salt, potassium salt, bromide, iodide, acetate. According to a preferred embodiment, the thermal oxidant is a combination of multiple different species. For example, in a preferred embodiment, the thermal oxidant is cupric acetate / cuprous iodide / potassium iodide, or cupric acetate / cuprous bromide / potassium bromide.

[0111] The amount of the thermal oxidation inhibitor depends on the desired final product properties. For example, the content of the thermal oxidation inhibitor in the raw material of the resin of the first aspect of the present application is 0 to 1 weight %, or 0.01 to 1 weight %, or 0.02 to 1 weight %, or 0.05 to 1 weight %, or 0.1 to 1 weight %, or 0.15 to 1 weight %, or 0.2 to 1 weight %, or 0.3 to 1 weight %, or 0.4 to 1 weight %, or 0.5 to 1 weight %, or 0.6 to 1 weight %, or 0.7 to 1 weight %, or 0.8 to 1 weight %, or 0.9 to 1 weight %, relative to the total weight of component a) and component b).

[0112] Multifunctional stabilizer

[0113] According to a preferred embodiment, the raw material of the resin in the first aspect of the present application further includes component g) a multifunctional stabilizer.

[0114] In the context of the present application, the term "multifunctional stabilizer" has the same meaning as commonly understood by those skilled in the art.

[0115] The multifunctional stabilizer is not particularly limited. In a non-limiting example, the multifunctional stabilizer is selected from di(2,2,6,6-tetramethyl-3-piperidinylamino)-isophthalamide and its derivatives.

[0116] The content of the multifunctional stabilizer depends on the desired final product quality. In a non-limiting embodiment, the content of the multifunctional stabilizer in the raw material of the resin of the first aspect of the present application is 0 to 1 weight %, or 0.01 to 1 weight %, or 0.02 to 1 weight %, or 0.05 to 1 weight %, or 0.07 to 1 weight %, or 0.1 to 1 weight %, or 0.2 to 1 weight %, or 0.3 to 1 weight %, or 0.4 to 1 weight %, or 0.5 to 1 weight %, or 0.6 to 1 weight %, or 0.7 to 1 weight %, or 0.7 to 1 weight %, or 0.8 to 1 weight %, or 0.9 to 1 weight %, relative to the total weight of component a) and component b).

[0117] The second aspect of the present application relates to a method for preparing the resin of the first aspect of the present application, the method comprising the following steps:

[0118] i) mixing adipic acid and hexamethylenediamine and dissolving them in water;

[0119] ii) adding comonomers and processing aids to the mixture obtained in step i);

[0120] iii) subjecting the mixture obtained in step ii) to polymerization.

[0121] The comonomer and processing aid are as described in the first aspect of the present application.

[0122] According to a preferred embodiment, step i) of the method of the second aspect of the present application comprises the following sub-steps:

[0123] i-1) mixing adipic acid and hexamethylenediamine in a molar ratio of 1:1 and dissolving in water;

[0124] i-2) The pH of the solution is adjusted to 6.90 to 7.90 with adipic acid or hexamethylenediamine.

[0125] In step i-1), a 66 salt solution is formed. Step i-1) can be performed under suitable conditions. As a non-limiting example, step i-1) can be performed at 50 to 70° C., and the mixing time can be 20 to 50 min.

[0126] The concentration of the 66 salt solution obtained in step i-1) can be selected as needed. As a non-limiting example, the amount of water can be controlled so that the concentration of the 66 salt solution obtained in step i-1) is 42 to 65% by weight.

[0127] According to a preferred embodiment, the above step ii) further comprises adding one or more of a promoter, a thermal oxidation inhibitor, and a multifunctional stabilizer.

[0128] The accelerator, thermal oxidation inhibitor and multifunctional stabilizer are as described in the first aspect.

[0129] According to a preferred real-time method, step iii) of the method of the second aspect of the present application includes the following sub-steps:

[0130] iii-1) concentrating the product obtained in step ii) at a first temperature T1 and a first pressure p1;

[0131] iii-2) optionally further concentrating the product obtained in step iii-1) at a second temperature T2 and a second pressure p2;

[0132] iii-3) performing a polymerization reaction at a third temperature T3 and a third pressure p3.

[0133] The above temperature and pressure can be selected according to actual needs.

[0134] According to a non-limiting embodiment, in sub-step iii-1), T1 ranges from 130 to 160° C., and p1 ranges from 0.15 to 0.20 MPa. The duration of sub-step iii-1) can be adjusted according to the type and concentration of the reactants. In one embodiment, sub-step iii-1) can be performed for 60 to 90 min.

[0135] According to a non-limiting embodiment, sub-step iii-2) is present, and wherein T2 ranges from 230 to 250° C., and p2 ranges from 1.70 to 1.90 MPa. The duration of sub-step iii-2) may be, for example, from 40 to 80 min.

[0136] According to a non-limiting embodiment, in sub-step iii-3), T3 ranges from 260 to 290° C., and p3 ranges from −0.08 to −0.02 MPa (relative pressure). The duration of sub-step iii-3) may be, for example, 10 to 30 min.

[0137] According to a non-limiting embodiment, in the product obtained in sub-step iii-1), the content of 66 salt formed by adipic acid and hexamethylenediamine is 75 to 90 weight %, relative to the total weight of the product obtained in sub-step iii-1).

[0138] The concentration process of sub-step iii-1) and optional sub-step iii-2) can be carried out using methods well known to those skilled in the art. For example, sub-step iii-1) and optional sub-step iii-2) can be carried out directly in the polymerization reactor carrying out step iii-3).

[0139] The resin of the first aspect of the present application or the resin obtained by the method of the second aspect of the present application can be used directly, or after post-treatment (such as purification, blending, etc.), used alone or in combination with other materials.

[0140] The third aspect of the present application relates to a composition comprising the resin described in the first aspect of the present application, or a resin prepared by the method of the second aspect of the present application.

[0141] As a non-limiting example, the composition may be a polymer alloy of PA66 and other materials.

[0142] The fourth aspect of the present application relates to a product prepared from the resin described in the first aspect of the present application or the composition described in the third aspect of the present application.

[0143] In a preferred embodiment, the product of the fourth aspect of the present application is selected from: fibers, automobile housings, electronic and electrical housings, gears, bearings, ropes, conveyor belts, parachutes, tire cord fabrics, fibers for textiles and clothing, food packaging bags, and medical packaging bags.

[0144] The present application provides a method for preparing a high-strength and high-elongation-at-break polyamide 66 resin. The method is simple and easy to implement, has significant effects, and can effectively improve the elongation at break and the notched impact strength while maintaining the intrinsic high-strength and high-modulus mechanical properties.

[0145] Therefore, the fifth aspect of the present application relates to the use of the combination of the comonomer and the processing aid as described above for improving the elongation at break of PA66 resin; the sixth aspect of the present application relates to the use of the combination of the comonomer and the processing aid as described above for improving the elongation at break of PA66 resin.

[0146] The high-strength and high-elongation-at-break polyamide 66 resin of the present application can be widely used in engineering plastics such as automobile housings, electronic and electrical housings, gears, bearings, and fiber fields such as ropes, transmission belts, parachutes, cord fabrics, textiles and clothing.

[0147] Compared with the prior art, the present invention has at least the following beneficial effects:

[0148] (1) The polyamide 66 resin not only maintains high-strength intrinsic mechanical properties, but also has satisfactory tensile strength, elongation at break and notched impact strength. This high strength and high elongation at break property can significantly improve the toughness of polyamide 66 plastic products and improve the flexibility and processability of polyamide 66 fiber products.

[0149] (2) The raw materials are cheap and readily available, the preparation process is simple and reliable, and the traditional polyamide 66 polymerization process can be used. The comonomers and processing aids can be directly added into the polymerization process.

[0150] Example

[0151] To make the technical solution of the present invention clearer, the technical solution of the present invention will be further described below in conjunction with some specific embodiments. The described embodiments are intended to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention.

[0152] The raw materials used in the examples and comparative examples of the present application are as follows:

[0153] Hexamethylenediamine: provided by Ningxia Ruitai Technology Co., Ltd.

[0154] Adipic acid: provided by Shenma Industrial Co., Ltd.;

[0155] 2,2-Dimethylsuccinic acid: provided by Shanghai MacLean Biochemical Technology Co., Ltd.;

[0156] 1,3-Bis(aminomethyl)cyclohexane: provided by Shanghai MacLean Biochemical Technology Co., Ltd.;

[0157] Benzylsuccinic acid: provided by Leyan Reagents;

[0158] 1,2,2-Trimethyl-1,3-cyclopentanedicarboxylic acid: provided by Shanghai MacLean Biochemical Technology Co., Ltd.;

[0159] Manganese hypophosphite: provided by Shanghai McLean Biochemical Technology Co., Ltd.;

[0160] Copper acetate: brand PZSTAB, provided by Shanghai Puzhan Industrial Co., Ltd.;

[0161] Cuprous iodide: brand S5050, provided by Shanghai Puzhan Industrial Co., Ltd.;

[0162] Potassium iodide: brand S5070A, provided by Shanghai Puzhan Industrial Co., Ltd.;

[0163] SEED: Brand name SEED, provided by Clariant Chemical Technology (Shanghai) Co., Ltd.

[0164] TFB117: Brand TFB117, provided by Clariant Chemical Technology (Shanghai) Co., Ltd.

[0165] Calcium montanate: brand LICOMONT CAV 102P, provided by Clariant Chemical Technology (Shanghai) Co., Ltd.;

[0166] Ethylene bisoleamide: brand EBO-SPO, provided by Shenzhen Huayichang Chemical Pigment Co., Ltd.;

[0167] Pentaerythritol stearate: brand PETs-3976, provided by Shenzhen Huayichang Chemical Pigment Co., Ltd.;

[0168] Rice bran wax: brand LICOCARE RBW 360P VITA, provided by Clariant Chemical Technology (Shanghai) Co., Ltd.

[0169] Aluminum Stearate: Supplied by Hair Chemicals.

[0170] The test conditions of the experimental results in the examples and comparative examples of the present application are as follows:

[0171] - Test the relative viscosity of polyamide 66 resin according to HG / T 4182-2012

[0172] - Test the terminal amine groups of polyamide 66 resin according to HG / T 4182-2012;

[0173] -Injection molding of polyamide 66 resin according to GB / T 17037.1-2019;

[0174] -Test the tensile properties of injection molded specimens according to GB / T 1040-1992;

[0175] -Test the notched Izod impact strength of injection molded specimens according to GB / T 1843-2008.

[0176] Embodiment 1:

[0177] 3102.5g hexamethylenediamine and 3905.1g adipic acid were dissolved in 7003.6g pure water and stirred for 30 minutes to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 7g of comonomer 2,2-dimethylsuccinic acid, 0.07g of manganese hypophosphite, 0.63g of copper acetate, 7.05g of cuprous iodide, 6.75g of potassium iodide, 4.20g of SEED and 14g of calcium montanate are stirred evenly; the salt solution is transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle is controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature is raised to 230 to 250°C, and the pressure in the kettle is controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure is gradually reduced to normal pressure in the kettle; the negative pressure is pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction is carried out for 13 to 20min to prepare polyamide 66 resin.

[0178] Embodiment 2:

[0179] 3102.6g hexamethylenediamine and 3901.9g adipic acid were dissolved in 7002.5g pure water and stirred for 30 minutes to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 21g comonomer 2,2-dimethylsuccinic acid, 0.07g manganese hypophosphite, 0.63g copper acetate, 7.05g cuprous iodide, 6.75g potassium iodide, 8.20g SEED and 14g ethylene bisoleamide were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0180] Embodiment 3:

[0181] 3101.1g hexamethylenediamine and 3902.7g adipic acid were dissolved in 7000.5g pure water and stirred for 30 minutes to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.50; 21g comonomer 2,2-dimethylsuccinic acid, 0.07g manganese hypophosphite, 0.63g copper acetate, 7.05g cuprous iodide, 6.75g potassium iodide, 8.20g SEED and 14g ethylene bisoleamide were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0182] Embodiment 4:

[0183] 3100.2g hexamethylenediamine and 3902.2g adipic acid were dissolved in 7004.8g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.00; 21g comonomer 1,3-bis(aminomethyl)cyclohexane, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 14g ethylene bisoleamide were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0184] Embodiment 5:

[0185] 3099.3g hexamethylenediamine and 3904.1g adipic acid were dissolved in 7003.2g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 21g comonomer benzylsuccinic acid, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 14g of pentaerythritol stearate were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0186] Embodiment 6:

[0187] 3102.6g hexamethylenediamine and 3900.4g adipic acid were dissolved in 7003.7g pure water and stirred for 30 minutes to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 14g comonomer benzylsuccinic acid, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 28g of pentaerythritol stearate were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0188] Embodiment 7:

[0189] 3103.6g hexamethylenediamine and 3901.7g adipic acid were dissolved in 7005.0g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 14g comonomer 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 0.07g manganese hypophosphite, 1.26g cupric acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 28g rice bran wax (brand LICOCARE RBW 360P) were added. VITA, provided by Clariant Chemical Technology (Shanghai) Co., Ltd.) was stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18 MPa to drain and concentrate; after the end, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90 MPa to continue draining for 40 to 50 minutes; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02 MPa, and the reaction was carried out for 13 to 20 minutes to prepare polyamide 66 resin.

[0190] Embodiment 8:

[0191] 3103.1g hexamethylenediamine and 3899.5g adipic acid were dissolved in 7002.9g pure water and stirred for 30 minutes to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 7g of comonomer 2,2-dimethylsuccinic acid and 7g of comonomer 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 28g aluminum stearate were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0192] Embodiment 9:

[0193] 3102.2g hexamethylenediamine and 3903.4g adipic acid were dissolved in 7000.7g pure water and stirred for 30 minutes to form salt; an appropriate amount of hexamethylenediamine was added to adjust the pH value of the salt solution to 7.80; 7g of comonomer 2,2-dimethylsuccinic acid and 21g of comonomer 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 28g aluminum stearate were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0194] Embodiment 10:

[0195] 3100.3g hexamethylenediamine and 3905.6g adipic acid were dissolved in 7006.3g pure water and stirred for 30 minutes to form salt; an appropriate amount of hexamethylenediamine was added to adjust the pH value of the salt solution to 7.80; 35g of comonomer 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 0.07g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g TFB117 and 28g of pentaerythritol stearate were stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled at 0.16 to 0.18 MPa to drain and concentrate; after completion, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled at 1.70 to 1.90 MPa to continue draining for 40 to 50 minutes; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02 MPa, and the reaction was carried out for 13 to 20 minutes to prepare polyamide 66 resin.

[0196] Comparative Example 1:

[0197] 3102.4g hexamethylenediamine and 3902.9g adipic acid were dissolved in 7004.1g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.10; 0.14g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide and 8.20g SEED were added and stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled to 0.16 to 0.18MPa to drain and concentrate; after the end, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled to 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0198] Comparative Example 2:

[0199] 3101.5g hexamethylenediamine and 3903.7g adipic acid were dissolved in 7002.7g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.30; 7g comonomer 2,2-dimethylsuccinic acid, 0.14g manganese hypophosphite, 1.26g cupric acetate, 14.10 cuprous iodide, 13.50g potassium iodide, and 8.20g SEED were added and stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled to 0.16 to 0.18MPa to drain and concentrate; after the end, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled to 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0200] Comparative Example 3:

[0201] 3104.2g hexamethylenediamine and 3902.9g adipic acid were dissolved in 7004.8g pure water and stirred for 30min to form salt; an appropriate amount of adipic acid was added to adjust the pH value of the salt solution to 7.10; 0.14g manganese hypophosphite, 1.26g copper acetate, 14.10 cuprous iodide, 13.50g potassium iodide, 8.20g SEED and 14g pentaerythritol stearate were added and stirred evenly; the salt solution was transferred to a polymerization kettle, heated to 130 to 160°C, and the pressure in the kettle was controlled to 0.16 to 0.18MPa to drain and concentrate; after the end, the temperature was raised to 230 to 250°C, and the pressure in the kettle was controlled to 1.70 to 1.90MPa to continue draining for 40 to 50min; then the pressure was gradually reduced to normal pressure in the kettle; the negative pressure was pumped to a vacuum degree of -0.08 to -0.02MPa, and the reaction was carried out for 13 to 20min to prepare polyamide 66 resin.

[0202] The properties of the polyamide resins synthesized in the comparative examples are shown in Table 1:

[0203] Table 1

[0204]

[0205] The results of the examples and comparative examples of the present application show that the comonomer and the processing aid produce a synergistic effect, which significantly improves the elongation at break and the notched impact strength of the resin.

[0206] In terms of elongation at break, Comparative Example 1 uses neither comonomer nor processing aid, and the elongation at break (EB) of the PA66 obtained is 3.9%. Comparative Example 3 uses no comonomer but uses processing aid, and the increase in elongation at break of PA66 due to the use of processing aid is Δ EB (Processing aid) = 4.3%. Comparative Example 2 did not use a processing aid but used a comonomer. The elongation at break of PA66 obtained by using the comonomer was increased by Δ EB (comonomer) = 6.8%. If the incremental elongation at break brought by the processing aid and the comonomer are linearly added, a person skilled in the art would estimate that the incremental elongation at break brought by the use of the processing aid and the comonomer is Δ EB (Processing aid)+Δ EB (comonomer) = 11.1%, that is, the elongation at break of PA66 is 15% (3.9 + 11.1). This value is significantly lower than the elongation at break in Examples 1 to 10.

[0207] It can be seen that the increase in elongation at break of PA66 caused by the simultaneous use of processing aids and comonomers Δ EB(processing aid + comonomer) is significantly greater than the linear sum of the elongation at break caused by the processing aid and the comonomer, that is,

[0208] Δ EB (processing aid + comonomer)>Δ EB (Processing aid)+Δ EB (Comonomer)

[0209] It can be seen from the above results that the processing aid and the comonomer achieve a synergistic effect in improving the elongation at break of PA66 resin.

[0210] As for the notched impact strength of PA66 resin, in Comparative Example 1, neither comonomer nor processing aid was used, and the notched impact strength (IS) of the obtained PA66 was 4.67 KJ / m 2 Comparative Example 3 did not use a comonomer but used a processing aid. The increase in the notched impact strength of PA66 due to the use of the processing aid was Δ IS (Processing aid) = 0.26KJ / m 2 Comparative Example 2 did not use a processing aid but used a comonomer. The PA66 notched impact strength was increased by Δ IS (comonomer) = 0.46KJ / m 2 If the notched impact strength increments brought by the processing aid and the comonomer are linearly added, then a person skilled in the art would estimate that the notched impact strength increment brought by the use of the processing aid and the comonomer is Δ IS (Processing aid)+Δ IS (comonomer) = 0.72KJ / m 2 , that is, the notched impact strength of PA66 is expected to be 5.4 (4.67 + 0.72). This value is less than 6KJ / m 2 However, the notched impact strength of the PA66 resin in Examples 1 to 10 is significantly greater than 6 KJ / m 2 .

[0211] It can be seen that the increase in notched impact strength of PA66 caused by the simultaneous use of processing aids and comonomers Δ IS (processing aid + comonomer) is significantly greater than the linear sum of the notched impact strength increments brought by the processing aid and the comonomer, that is,

[0212] Δ IS (processing aid + comonomer)>Δ IS (Processing aid)+Δ IS (Comonomer)

[0213] It can be seen from the above results that the processing aid and the comonomer achieve a synergistic effect in improving the notched impact strength of PA66 resin.

[0214] The experimental results of the embodiments and comparative examples show that the present application provides a simple and feasible PA66 preparation method, which can use the traditional polyamide 66 polymerization process. The comonomer and the processing aid produce a synergistic effect, so that the polyamide 66 resin obtained in the present application has greatly improved the elongation at break and the notched impact strength while maintaining high tensile strength.

[0215] The PA66 resin of the present application can be widely used in engineering plastic fields such as automobile housings, electronic and electrical housings, gears, bearings, and fiber fields such as ropes, transmission belts, parachutes, cord fabrics, textiles and clothing.

[0216] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A resin prepared from a raw material comprising: a) adipic acid; b) hexamethylenediamine; c) comonomers; d) processing aids; wherein the comonomer is selected from the group consisting of C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines, with the proviso that the comonomer is different from adipic acid or hexamethylenediamine, and The processing aid is selected from the group consisting of fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof; Preferably, the comonomer content in the feedstock is 0.001 to 2 wt%, or 0.001 to 1.8 wt%, or 0.001 to 1.6 wt%, or 0.001 to 1.4 wt%, or 0.001 to 1.2 wt%, or 0.001 to 1.0 wt%, or 0.001 to 0.8 wt%, or 0.001 to 0.6 wt%, or 0.001 to 0.4 wt%, or 0.001 to 0.2 wt%, relative to the total weight of component a) and component b); and / or Preferably, the content of the processing aid in the raw material is 0.001 to 2% by weight, or 0.001 to 1.8% by weight, or 0.001 to 1.6% by weight, or 0.001 to 1.4% by weight, or 0.001 to 1.2% by weight, or 0.001 to 1.0% by weight, or 0.001 to 0.8% by weight, or 0.001 to 0.6% by weight, or 0.001 to 0.4% by weight, or 0.001 to 0.3% by weight, or 0.001 to 0.2% by weight, or 0.001 to 0.1% by weight, relative to the total weight of component a) and component b); and / or The fatty acid in the fatty acid ester, fatty acid salt, and fatty acid amide is selected from C2 to C30 fatty acids; and / or The fatty acid ester is an ester of a fatty acid and a C2 to C30 alcohol; preferably, the alcohol is selected from aliphatic monohydric alcohols, aliphatic polyhydric alcohols, and alicyclic polyhydric alcohols; and / or The fatty acid salt is an alkali metal salt, alkaline earth metal salt, aluminum salt, or transition metal salt of a fatty acid; more preferably, the fatty acid salt is selected from acetate, myristate, palmitate, oleate, stearate, isostearate, behenate, or montanate; and / or The fatty acid amide is selected from aliphatic monocarboxylic acid amides, N-substituted aliphatic monocarboxylic acid amides, aliphatic dicarboxylic acid amides, N-substituted aliphatic carboxylic acid bisamides, and N-substituted ureas; Particularly preferably, the processing aid is selected from pentaerythritol stearate, ethylene bisoleamide, rice bran wax, aluminum stearate, calcium montanate, sodium montanate, or a combination thereof.

2. The resin according to claim 1, wherein (i) the comonomer is selected from C3 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 aliphatic diacids, which may be optionally substituted with one or more of C1 to C12 hydrocarbon groups substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl; Preferably, the comonomer is selected from the group consisting of malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, 2-methylmalonic acid, 2,2-dimethylmalonic acid, 2-methylsuccinic acid, 2-butylsuccinic acid, 2-cyclohexylsuccinic acid, 2-acetylsuccinic acid, 2-p-tolylsuccinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylsuccinic acid, phenylsuccinic acid, benzylsuccinic acid, 2-methylglutaric acid, 3-methylglutaric acid, 2,2-dimethylglutaric acid, 2,4-diethylglutaric acid, 3,3-dimethylglutaric acid, 3,3-tetramethyleneglutaric acid, 3-ethyl-3-methylglutaric acid; and / or (ii) the comonomer is selected from a C4 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 alicyclic diacids, which may be optionally substituted with one or more of a C1 to C12 hydrocarbon group substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl; Preferably, the comonomer is selected from the group consisting of cyclopentanedicarboxylic acid, cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, cyclooctanedicarboxylic acid, cyclononanedicarboxylic acid, cyclodecanedicarboxylic acid, decahydronaphthalene dicarboxylic acid, 1,2,2-trimethyl-1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid; and / or (iii) the comonomer is selected from C3 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 aliphatic diamines, which may be optionally substituted with one or more of C1 to C12 hydrocarbon groups substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl; Preferably, the comonomer is selected from the group consisting of propylene diamine, butylene diamine, pentane diamine, hexane diamine, heptane diamine, octanediamine, nonane diamine, decane diamine, undecane diamine, dodecane diamine, 2-methylpropylene diamine, 2,2-dimethylpropylene diamine, 2-methylbutylene diamine, 2-butylbutylene diamine, 2-cyclohexylbutylene diamine, 2-acetylbutylene diamine, 2-p-tolylbutylene diamine, 2,2-dimethylbutylene diamine, 2,3-dimethylbutylene diamine, phenylbutylene diamine, benzylbutylene diamine, 2-methylpentane diamine, 3-methylpentane diamine, 2,2-dimethylpentane diamine, 2,4-diethylpentane diamine, 3,3-dimethylpentane diamine, 3,3-tetramethylenepentane diamine, 3-ethyl-3-methylpentane diamine; and / or (iv) the comonomer is selected from C4 to C12, preferably C4 to C12, preferably C5 to C12, preferably C6 to C12, preferably C7 to C12, preferably C8 to C12, preferably C9 to C12, preferably C10 to C12, preferably C11 to C12 alicyclic diamines, which may be optionally substituted with one or more of C1 to C12 hydrocarbon groups substituted with hydroxyl, halogen, amino, amine, thiol, C1 to C12 alkoxy, C1 to C12 acyl, C3 to C12 aryl, C3 to C12 aralkyl, C3 to C12 alkaryl, or C3 to C12 heteroaryl; Preferably, the comonomer is selected from: cyclopentanediamine, cyclohexanediamine, cycloheptanediamine, cyclooctanediamine, cyclononanediamine, cyclodecanediamine, decahydronaphthalenediamine, isophoronediamine, 1,2,2-trimethyl-1,3-cyclopentanediamine, 1,3-cyclohexanediamine, 1,3-bis(aminomethyl)cyclohexane, 2-aminocyclopentylmethylamine.

3. The resin according to claim 1, wherein: i) the number of moles of adipic acid of component a) is greater than the number of moles of hexamethylenediamine of component b), preferably the molar ratio of component a) to component b) is 1 to 1.1, or 1 to 1.09, or 1 to 1.08, or 1 to 1.07, or 1 to 1.06, or 1 to 1.05, or 1 to 1.04, or 1 to 1.03, or 1 to 1.02, or 1 to 1.01, or 1 to 1.005, or 1 to 1.001, or 1 to 1.0005, or 1 to 1.0001; or ii) wherein the number of moles of adipic acid of component a) is less than the number of moles of hexamethylenediamine of component b), preferably the molar ratio of component a) to component b) is from 0.9 to 1, or from 0.91 to 1, or from 0.92 to 1, or from 0.93 to 1, or from 0.94 to 1, or from 0.95 to 1, or from 0.96 to 1, or from 0.97 to 1, or from 0.98 to 1, or from 0.99 to 1, or from 0.995 to 1, or from 0.999 to 1, or from 0.9995 to 1, or from 0.9999 to 1.

4. The resin according to claim 1, wherein the raw material further comprises one or more of the following: e) Accelerator. Preferably, the accelerator is selected from hypophosphites, preferably manganese hypophosphite and magnesium hypophosphite; Preferably, the content of the accelerator is 1 to 500 ppm by weight, or 1 to 450 ppm by weight, or 1 to 400 ppm by weight, or 1 to 350 ppm by weight, or 1 to 300 ppm by weight, or 1 to 250 ppm by weight, or 1 to 200 ppm by weight, or 1 to 150 ppm by weight, or 1 to 100 ppm by weight, or 1 to 80 ppm by weight, or 1 to 60 ppm by weight, or 1 to 40 ppm by weight, or 1 to 20 ppm by weight, relative to the total weight of component a) and component b); f) Thermal oxidant Preferably, the thermal antioxidant is selected from: copper salts, cuprous salts, potassium salts, bromides, iodides, acetates, preferably, the thermal antioxidant is selected from cupric acetate / cuprous iodide / potassium iodide, cupric acetate / cuprous bromide / potassium bromide; Preferably, the content of the thermal oxidation inhibitor in the raw material is 0 to 1% by weight, or 0.01 to 1% by weight, or 0.02 to 1% by weight, or 0.05 to 1% by weight, or 0.1 to 1% by weight, or 0.15 to 1% by weight, or 0.2 to 1% by weight, or 0.3 to 1% by weight, or 0.4 to 1% by weight, or 0.5 to 1% by weight, or 0.6 to 1% by weight, or 0.7 to 1% by weight, or 0.8 to 1% by weight, or 0.9 to 1% by weight, relative to the total weight of component a) and component b); g) Multifunctional stabilizer Preferably, the multifunctional stabilizer is selected from di(2,2,6,6-tetramethyl-3-piperidinylamino)-isophthalamide and its derivatives; Preferably, the content of the multifunctional stabilizer in the raw material is 0 to 1 wt%, or 0.01 to 1 wt%, or 0.02 to 1 wt%, or 0.05 to 1 wt%, or 0.07 to 1 wt%, or 0.1 to 1 wt%, or 0.2 to 1 wt%, or 0.3 to 1 wt%, or 0.4 to 1 wt%, or 0.5 to 1 wt%, or 0.6 to 1 wt%, or 0.7 to 1 wt%, or 0.7 to 1 wt%, or 0.8 to 1 wt%, or 0.9 to 1 wt%, relative to the total weight of component a) and component b).

5. A method for preparing a resin as claimed in any one of claims 1 to 4, comprising the steps of: i) mixing adipic acid and hexamethylenediamine and dissolving them in water; Preferably, step i) comprises the following sub-steps: i-1) mixing adipic acid and hexamethylenediamine in a molar ratio of 1:1 and dissolving in water; i-2) adjusting the pH of the solution to 6.90 to 7.90 with adipic acid or hexamethylenediamine; ii) adding comonomers and processing aids to the mixture obtained in step i); iii) subjecting the mixture obtained in step ii) to polymerization; wherein the comonomer is selected from the group consisting of C2 to C12 aliphatic diacids, C3 to C12 alicyclic diacids, C2 to C12 aliphatic diamines, and C3 to C12 alicyclic diamines, with the proviso that the comonomer is different from adipic acid or hexamethylenediamine, and The processing aid is selected from the group consisting of fatty acid esters, fatty acid salts, fatty acid amides, or mixtures thereof; Preferably, step ii) further comprises adding one or more of a promoter, a thermal oxidation inhibitor, and a multifunctional stabilizer; and / or Step iii) comprises the following sub-steps: iii-1) concentrating the product obtained in step ii) at a first temperature T1 and a first pressure p1; preferably, T1 ranges from 130 to 160° C., and p1 ranges from 0.15 to 0.20 MPa; preferably, the content of 66 salt formed by adipic acid and hexamethylenediamine in the product obtained by iii-1) is 75 to 90% by weight, relative to the total weight of the product obtained by iii-1); iii-2) optionally further concentrating the product obtained in step iii-1) at a second temperature T2 and a second pressure p2; preferably, T2 ranges from 230 to 250° C., and p2 ranges from 1.70 to 1.90 MPa; iii-3) carrying out polymerization at a third temperature T3 and a third pressure p3; preferably T3 is in the range of 260 to 290°C, and p3 is in the range of -0.08 to -0.02 MPa (relative pressure).

6. The method according to claim 5, wherein in step i), (1) the number of moles of adipic acid is greater than the number of moles of hexamethylenediamine, preferably the molar ratio of adipic acid to hexamethylenediamine is 1 to 1.1, or 1 to 1.09, or 1 to 1.08, or 1 to 1.07, or 1 to 1.06, or 1 to 1.05, or 1 to 1.04, or 1 to 1.03, or 1 to 1.02, or 1 to 1.01, or 1 to 1.005, or 1 to 1.001, or 1 to 1.0005, or 1 to 1.0001; or (2) The molar number of adipic acid is less than the molar number of hexamethylenediamine, and preferably the molar ratio of adipic acid to hexamethylenediamine is 0.9 to 1, or 0.91 to 1, or 0.92 to 1, or 0.93 to 1, or 0.94 to 1, or 0.95 to 1, or 0.96 to 1, or 0.97 to 1, or 0.98 to 1, or 0.99 to 1, or 0.995 to 1, or 0.999 to 1, or 0.9995 to 1, or 0.9999 to 1.

7. A composition comprising a resin as claimed in any one of claims 1 to 4 or a resin prepared by a process as claimed in any one of claims 5 to 6.

8. An article prepared from the resin according to any one of claims 1 to 4 or the composition according to claim 7; Preferably, the product is selected from: fibers, automobile housings, electronic and electrical housings, gears, bearings, ropes, conveyor belts, parachutes, tire cord fabrics, fibers for textiles and clothing, food packaging bags, and medical packaging bags.

9. Use of the combination of a comonomer and a processing aid as defined in claims 1 to 4 for increasing the elongation at break of PA66 resin.

10. Use of the combination of comonomer and processing aid as defined in claims 1 to 4 for improving the notched impact strength of PA66 resin.

Citation Information

Cited By

  • Polyamide composite material as well as preparation method and application thereof

    CN120082197A

  • Polyamide composite material, method for producing same, and use thereof

    CN120082197B

  • Long-chain polyamide resin easy to process and high in tensile property as well as preparation method and application of long-chain polyamide resin

    CN120518853A

  • A long-chain polyamide resin with easy processability and high tensile property, and a preparation method and application thereof

    CN120518853B