Thermosetting polyimide resin, preparation method thereof and composite material
By introducing flexible ether bonds and large-volume fluorene-based structures into thermosetting polyimide resins, the problems of polyimide resin’s contradiction between heat resistance and toughness and poor processing performance are solved, achieving high solubility, low viscosity and high Tough resin, suitable for low-cost molding process to prepare high-quality composite materials.
Patent Information
- Application Number
- CN202411034019.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Existing thermosetting polyimide resins have conflicts between heat resistance and toughness, poor processability, high resin melt viscosity and insufficient material toughness after curing, making it difficult to prepare high-quality composite materials through low-cost molding processes.
Thermosetting polyimide resin is prepared by using ether-containing fluorene dianhydride monomer, introducing flexible ether bonds and large-volume fluorene-based structure, and synthesizing it under a protective atmosphere through a one-step reaction, which reduces the viscosity of the resin melt and improves the toughness, while having good Heat resistance and processability.
It achieves high solubility and low viscosity of thermosetting polyimide resin in polar aprotic solvents. The cured product has high heat resistance and high toughness. It is suitable for the preparation of low-porosity composite materials by low-cost molding process and solves the problem of existing technologies. The problem of insufficient processability and toughness of composite materials.
Smart Images

Figure CN118755086A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of synthesis of high-performance polymer materials, and in particular relates to a high-toughness, easy-to-process, high-temperature-resistant thermosetting polyimide resin and a preparation method and a composite material thereof. Background Art
[0002] Thermosetting polyimide is a type of polymer material that contains active end groups in the prepolymer structure. After cross-linking and curing, the resin contains a three-dimensional network structure. It has good heat resistance, mechanical properties and dielectric properties, and is widely used in many fields such as aerospace, mechanical chemical industry, and microelectronics. However, due to the rigid structure of polyimide, it has strong intramolecular / intermolecular forces. These factors make the polyimide resin insoluble and non-meltable after imidization, and the processability is poor. Therefore, the preparation of its composite materials is mostly completed by impregnating fibers with polyamic acid or PMR solution precursors, which results in a large porosity of the composite material and requires the use of a costly autoclave process for preparation. On the other hand, the heat resistance of polyimide resins and their toughness are contradictory and difficult to have both. In the Chinese patent applications with publication numbers CN116574259A and CN114369243A and the article High performance imide oligomers and thermosets derived from 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride (Polymer 2023, 281, 126086), it is reported that the use of non-coplanar torsional rigid fluorene structures to synthesize polyimides makes the thermosetting polyimide resin have high solubility after imidization and the resin cured product has the characteristics of high heat resistance. However, the monomer used is a rigid fluorene structure, which is affected by the structural rigidity of the monomer itself, resulting in a high viscosity of the resin melt, poor processability, and insufficient toughness of the material after curing. Therefore, the development of high temperature resistant, high toughness, and easy-to-process soluble polyimide resins suitable for low-cost molding processes is a technical problem that needs to be solved urgently. So far, there has been no research on the use of ether-containing fluorene dianhydride monomers to prepare thermosetting polyimide resins. Summary of the invention
[0003] In order to solve the above-mentioned problems of the prior art, the present invention provides a thermosetting polyimide resin and a preparation method and a composite material thereof, so as to overcome a series of technical difficulties such as the contradiction between heat resistance and toughness of the existing polyimide resin, poor processing performance, high resin melt viscosity and insufficient toughness of the material after curing.
[0004] The present invention is achieved through the following technical solutions:
[0005] A thermosetting polyimide resin having a structure as shown in formula (I):
[0006]
[0007] Wherein, n is any positive number from 1 to 10, and each Ar is independently a structure represented by any of the following formulae:
[0008]
[0009] R is a structure represented by any of the following formulae:
[0010]
[0011] The dotted line represents the insertion position of the amino group.
[0012] Preferably, the dissolved solid content of the thermosetting polyimide resin in the polar aprotic solvent is greater than 30%;
[0013] And / or, the minimum melt viscosity of the thermosetting polyimide resin is 3 to 1254 Pa·s;
[0014] And / or, the cured product of the thermosetting polyimide resin has a glass transition temperature of 335 to 425° C.;
[0015] And / or, the cured product of the thermosetting polyimide resin has a 5% thermal weight loss temperature in air higher than 520° C. and an elongation at break higher than 2%.
[0016] The preparation method of the thermosetting polyimide resin comprises:
[0017] S1, under a protective atmosphere, mixing an aromatic diamine monomer, an ether-containing fluorene dianhydride monomer and an organic solvent, and reacting at 95-105° C. for 6-8 hours;
[0018] S2, adding a capping agent to the mixed reaction system obtained in step S1, and continuing the reaction at 95-105° C. for 2-4 hours;
[0019] S3, heating the reaction mixture obtained in step S2 to 195-205° C. and continuing the reaction for 4-6 hours;
[0020] S4, mixing the reaction mixture obtained in step S3 with a cleaning agent to precipitate a solid, and washing and drying the obtained solid to obtain a thermosetting polyimide resin.
[0021] Preferably, in step S1, the ether-containing fluorene anhydride monomer has a structure as shown in formula (II):
[0022]
[0023] Preferably, in step S1, the aromatic diamine monomer is any one of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 4,4'-[1,4-phenylbis(oxy)]bis[3-(trifluoromethyl)aniline], 1,3-phenylenediamine, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, [1,1':3',1"-terphenyl]-4,4"-diamine, [1,1':3',1"-terphenyl]-3,3"-diamine and [1,1':4',1"-terphenyl]-3,3"-diamine, or a combination of two or more thereof.
[0024] Preferably, in step S1, the molar ratio of the ether-containing fluorene dianhydride monomer, the aromatic diamine monomer and the end-capping agent is n:(n+1):2, wherein n>0.
[0025] Preferably, in step S1, the organic solvent is any one of m-cresol and sulfolane, or a combination of two or more thereof.
[0026] Preferably, in step S2, the end-capping agent is any one of 4-phenylethynylphthalic anhydride, ethynylphthalic anhydride and norbornene dicarboxylic anhydride;
[0027] And / or, in step S2, after adding the end-capping agent to the mixed reaction system obtained in step S1, the solid content in the obtained mixed solution is controlled to 20wt% to 40wt%, and the reaction is continued for 2 to 4h.
[0028] Preferably, in step S4, the cleaning agent is one or more of methanol, ethanol or deionized water;
[0029] And / or, in step S4, the drying temperature is 220-240°C.
[0030] The present invention also provides a polyimide resin-based composite material, comprising the thermosetting polyimide resin according to any one of claims 1 to 2.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] The thermosetting polyimide resin provided by the present invention contains a flexible ether bond and a large-volume rigid non-coplanar fluorene-based structure. The introduction of the flexible ether bond can improve the segment movement between the molecular chains, thereby reducing the resin melt viscosity and improving the toughness of the resin cured product. The large-volume fluorene-based structure can increase the molecular chain spacing, making it easier for solvent molecules to penetrate, and has the characteristics of a rigid structure. At the same time, the flexible ether bond and the rigid non-coplanar fluorene-based structure are on the same monomer, avoiding the problem of high resin melt viscosity caused by monomer rigidity, so that the polyimide resin It has high solubility and low viscosity. The cured resin has the characteristics of high temperature resistance and high toughness. The dissolved solid content in polar aprotic solvent is greater than 30%. The melt viscosity is adjustable within the range of 0 to 1500 Pa·s. The 5% thermal weight loss temperature of the cured polyimide resin in air is higher than 520°C, and the elongation at break is greater than 2%. Therefore, the thermosetting polyimide resin has good heat resistance, processability and mechanical toughness, and solves the technical problems of difficult processing and poor toughness of the matrix resin faced by the existing thermosetting polyimide composite materials. During the molding process of the composite material based on this type of resin, no small molecular volatiles are released at high temperature, and low-porosity and large-size and thick composite products can be prepared by low-cost molding process.
[0033] The preparation method of the present invention innovatively uses ether-containing fluorene dianhydride monomers to prepare thermosetting polyimide resins. The introduction of flexible ether bonds can improve the segment movement between molecular chains, thereby reducing the resin melt viscosity and improving the toughness of the resin cured product. The large-volume fluorene-based structure can increase the molecular chain spacing, making it easier for solvent molecules to penetrate, and has the characteristics of a rigid structure. At the same time, the flexible ether bond and the rigid non-coplanar fluorene-based structure are on the same monomer, avoiding the problem of high resin melt viscosity caused by monomer rigidity. The obtained polyimide resin has good heat resistance, processability and mechanical toughness. The method adopts a one-step method to directly complete the preparation of the polyimide resin in a reaction vessel without adding any dehydrating agent and catalyst, and the process is relatively simple. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0035] Figure 1 is the FT-IR spectrum of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0036] Figure 2 is a DSC curve diagram of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0037] Figure 3 is a rheological curve diagram of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0038] Figure 4 is a DMA curve diagram of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0039] Figure 5 is a TGA curve diagram of the cured product of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0040] Figure 6 is a mechanical property diagram of the thermosetting polyimide resin prepared in Example 1 of the present invention;
[0041] Figure 7 This is a diagram showing the solubility of the thermosetting polyimide resin prepared in Example 1 of the present invention in N-methylpyrrolidone, N,N-dimethylacetamide, tetrahydrofuran, and 1,4-dioxane. DETAILED DESCRIPTION
[0042] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] An embodiment of the present invention provides a thermosetting polyimide resin, wherein the thermosetting polyimide resin has a structure as shown in formula (I):
[0044]
[0045] Wherein, n is any positive number from 1 to 10, and each Ar is independently a structure shown in any of the following formulae, that is, Ar in each structural unit may be the same or different:
[0046]
[0047] R is a structure represented by any of the following formulae:
[0048]
[0049] The dotted line represents the insertion position of the amino group.
[0050] In the thermosetting polyimide resin of the present invention, R is preferably:
[0051]
[0052] The thermosetting polyimide resin of the present invention has a minimum melt viscosity of 3 to 1254 Pa·s; the glass transition temperature of the thermosetting polyimide resin cured product is 335 to 425°C; the dissolved solid content of the thermosetting polyimide resin in a polar aprotic solvent is greater than 30%; the 5% thermal weight loss temperature of the cured product of the thermosetting polyimide resin in air is higher than 520°C, and the elongation at break is greater than 2%. Wherein, the polar aprotic solvent is N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), tetrahydrofuran (DMF) or 1,4-dioxane (1,4-Dioxance).
[0053] The preparation method of the thermosetting polyimide resin of the present invention comprises:
[0054] S1, under a protective atmosphere, mixing an aromatic diamine monomer, an ether-containing fluorene dianhydride monomer and an organic solvent, and reacting at 95-105° C. for 6-8 hours;
[0055] S2, adding a capping agent to the mixed reaction system obtained in step S1, and continuing the reaction at 95-105° C. for 2-4 hours;
[0056] S3, heating the reaction mixture obtained in step S2 to 195-205° C. and continuing the reaction for 4-6 hours;
[0057] S4, pouring the reaction mixture obtained in step S3 into a cleaning agent and stirring and mixing the mixture sufficiently, filtering, washing and drying the solid after precipitation to obtain a thermosetting polyimide resin.
[0058] In some more specific embodiments, in step S1, the ether-containing fluorene anhydride monomer has a structure as shown in formula (II):
[0059]
[0060] In some more specific embodiments, in step S1, the aromatic diamine monomer is one or a combination of two or more of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 4,4'-[1,4-phenylbis(oxy)]bis[3-(trifluoromethyl)aniline], 1,3-phenylenediamine, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, [1,1':3',1"-terphenyl]-4,4"-diamine, [1,1':3',1"-terphenyl]-3,3"-diamine and [1,1':4',1"-terphenyl]-3,3"-diamine, and their structural formulas are shown in formulas (III) to (XI) in sequence:
[0061]
[0062] In some more specific embodiments, the molar ratio of the ether-containing fluorene dianhydride monomer, the aromatic diamine monomer and the capping agent is n:(n+1):2, wherein n>0.
[0063] In some more specific embodiments, in step S1, the organic solvent is any one of m-cresol and sulfolane or a combination of two or more thereof, but is not limited thereto.
[0064] In some more specific embodiments, in step S1, the protective atmosphere is a nitrogen atmosphere and / or an inert gas atmosphere.
[0065] Furthermore, the inert gas atmosphere is an argon atmosphere and / or a helium atmosphere, but is not limited thereto.
[0066] In some more specific embodiments, step S2 specifically includes: after the reaction in step S1 is completed, adding a capping agent to the obtained mixed reaction system, while controlling the solid content in the obtained mixed solution to 20wt% to 40wt%, and continuing the reaction for 2 to 4h.
[0067] In some more specific embodiments, in step S2, the end-capping agent is any one of 4-phenylethynylphthalic anhydride (4-PEPA), ethynylphthalic anhydride (4-EPA) and naphthalene dicarboxylic anhydride (NA). The structural formulas of 4-phenylethynylphthalic anhydride, ethynylphthalic anhydride and naphthalene dicarboxylic anhydride are shown in formulas (XII) to (XIV), respectively:
[0068]
[0069] In some more specific embodiments, in step S4, the drying temperature is 220-240°C.
[0070] In some more specific embodiments, in step S4, the theoretical degree of polymerization of the obtained thermosetting polyimide resin is 1-10.
[0071] Furthermore, in step S4, the cleaning agent is one or more of methanol, ethanol or deionized water, and the amount used is 5 to 10 times that of the organic solvent in step S1.
[0072] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0073] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.
[0074] Example 1
[0075] Under nitrogen protection, 5.6 g of [1,1':3',1"-terphenyl]-4,4"-diamine and 6.9116 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 30 g of m-cresol was added. The reaction was carried out at 95° C. for 6 h under mechanical stirring, and then 5.3399 g of 4-PEPA and 10 g of m-cresol were added. The solid content of the resulting solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 190° C. for 6 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 240° C. for 2 h to obtain a thermosetting polyimide resin as shown in formula (i).
[0076]
[0077] Structural characterization:
[0078] The thermosetting polyimide resin prepared in this embodiment has a dissolved solid content of 30% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 3 Pa·s, a glass transition temperature of 385° C., an elongation at break of 2.5%, and a 5% thermal weight loss temperature in air of 573° C.
[0079] Example 2
[0080] Under nitrogen protection, 8 g of 4,4'-[1,4-phenylbis(oxy)]bis[3-(trifluoromethyl)aniline] and 10.0018 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 40 g of sulfolane was added. The mixture was reacted at 100° C. for 6 h under mechanical stirring, and then 1.5455 g of 4-PEPA and 10 g of m-cresol were added. The solid content of the resulting solution was adjusted to 28 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. for 5 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 220° C. for 3 h to obtain a thermosetting polyimide resin as shown in formula (ii).
[0081]
[0082] Structural characterization:
[0083] The thermosetting polyimide resin prepared in this embodiment has a dissolved solid content of 33% in the polar aprotic solvent N,N-dimethylacetamide, a minimum melt viscosity of 205 Pa·s, a glass transition temperature of 342° C., an elongation at break of 4.0%, and a 5% thermal weight loss temperature in air of 572° C.
[0084] Example 3
[0085] Under nitrogen protection, 3 g of 1,3-phenylenediamine and 13.3704 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 45 g of m-cresol was added. The mixture was reacted at 100 ° C for 6 h under mechanical stirring, and then 3.4433 g of 4-PEPA and 15 g of m-cresol were added. The solid content of the resulting solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195 ° C for 4 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 240 ° C for 2 h to obtain a thermosetting polyimide resin as shown in formula (iii).
[0086]
[0087] Structural characterization:
[0088] The thermosetting polyimide resin prepared in this embodiment has a soluble solid content of 35% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 30 Pa·s, a glass transition temperature of 354° C., an elongation at break of 3.4%, and a 5% thermal weight loss temperature in air of 568° C.
[0089] Example 4
[0090] Under nitrogen protection, 6 g of 2,2'-dimethyl-4,4'-diaminobiphenyl and 13.6217 g of ether-containing fluorene anhydride monomer were added to a 250 ml reaction bottle and placed in an oil bath, and then 40 g of m-cresol was added. The reaction was carried out at 105° C. for 6 h under mechanical stirring, and then 3.5080 g of 4-PEPA and 20 g of m-cresol were added. The solid content of the obtained solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. for 6 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 220° C. for 4 h to obtain a thermosetting polyimide resin as shown in formula (iv).
[0091]
[0092] Structural characterization:
[0093] The thermosetting polyimide resin prepared in this embodiment has a dissolved solid content of 36% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 205 Pa·s, a glass transition temperature of the cured product of 381° C., an elongation at break of 3.5%, and a 5% thermal weight loss temperature in air of 563° C.
[0094] Example 5
[0095] Under nitrogen protection, 9 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether and 12.8996 g of ether-containing fluorene dianhydride monomer were added to a 250 ml reaction bottle and placed in an oil bath, and then 40 g of m-cresol was added. The reaction was carried out at 95° C. for 4 h under mechanical stirring, and then 3.3223 g of 4-PEPA and 18 g of m-cresol were added. The solid content of the resulting solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. for 5 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 230° C. for 2 h to obtain a thermosetting polyimide resin as shown in formula (v).
[0096]
[0097] Structural characterization:
[0098] The thermosetting polyimide resin prepared in this embodiment has a soluble solid content of 40% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 102 Pa·s, a glass transition temperature of 346°C, an elongation at break of 3.8%, and a 5% thermal weight loss temperature in air of 564°C.
[0099] Example 6
[0100] Under nitrogen protection, 4 g of 9,9-bis(4-aminophenyl)fluorene and 3.6885 g of ether-containing fluorene dianhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 15 g of m-cresol was added. The mixture was reacted at 100 ° C for 6 h under mechanical stirring, and then 2.8497 g of 4-PEPA and 8 g of m-cresol were added. The solid content of the resulting solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 200 ° C for 4 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 240 ° C for 2 h to obtain a thermosetting polyimide resin as shown in formula (vi).
[0101]
[0102] Structural characterization:
[0103] The thermosetting polyimide resin prepared in this embodiment has a dissolved solid content of 30% in the polar aprotic solvent 1,4-dioxane, a minimum melt viscosity of 485 Pa·s, a glass transition temperature of 425°C, an elongation at break of 2.8%, and a 5% thermal weight loss temperature in air of 568°C.
[0104] Example 7
[0105] Under nitrogen protection, 6 g of [1,1':3',1"-terphenyl]-3,3"-diamine and 13.1650 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 40 g of cyclopentane was added. The reaction was carried out at 95° C. for 4 h under mechanical stirring, and then 1.2714 g of 4-PEPA and 10 g of cyclopentane were added. The solid content of the resulting solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 200° C. and reacted for 4 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 240° C. for 2 h to obtain a thermosetting polyimide resin as shown in formula (vii).
[0106]
[0107] Structural characterization:
[0108] The thermosetting polyimide resin prepared in this embodiment has a soluble solid content of 35% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 1254 Pa·s, a glass transition temperature of 362° C., an elongation at break of 3.6%, and a 5% thermal weight loss temperature in air of 570° C.
[0109] Example 8
[0110] Under nitrogen protection, 8 g of 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl and 8.0268 g of ether-containing fluorene anhydride monomer were added to a 250 ml reaction bottle and placed in an oil bath, and then 40 g of m-cresol was added. The mixture was reacted at 100° C. for 4 h under mechanical stirring, and then 4.3004 g of EPA and 8 g of m-cresol were added. The solid content of the solution was adjusted to 30 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. and reacted for 6 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 230° C. for 2 h to obtain a thermosetting polyimide resin as shown in formula (viii).
[0111]
[0112] Structural characterization:
[0113] The thermosetting polyimide resin prepared in this embodiment has a dissolved solid content of 32% in the polar aprotic solvent 1,4-dioxane, a minimum melt viscosity of 57 Pa·s, a glass transition temperature of 342°C, an elongation at break of 2.6%, and a 5% thermal weight loss temperature in air of 535°C.
[0114] Example 9
[0115] Under nitrogen protection, 1.0097 g of 2,2'-dimethyl-4,4'-diaminobiphenyl, 2.9732 g of 1,3-phenylenediamine and 12 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 32 g of cyclopentane was added. The reaction was carried out at 95° C. for 4 h under mechanical stirring, and then 2.3178 g of 4-PEPA and 10 g of cyclopentane were added. The solid content of the solution was adjusted to 35 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. for 5 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 230° C. for 2 h to obtain a hot melt as shown in formula (ix):
[0116]
[0117] Structural characterization:
[0118] The thermosetting polyimide resin prepared in this embodiment has a soluble solid content of 40% in the polar aprotic solvent N,N-dimethylacetamide, a minimum melt viscosity of 16 Pa·s, a glass transition temperature of 387° C., an elongation at break of 3.2%, and a 5% thermal weight loss temperature in air of 555° C.
[0119] Example 10
[0120] Under nitrogen protection, 4.7571 g of 2,2'-dimethyl-4,4'-diaminobiphenyl and 12 g of ether-containing fluorene anhydride monomer were added to a 100 ml reaction bottle and placed in an oil bath, and then 38 g of m-cresol was added. The mixture was reacted at 100° C. for 4 h under mechanical stirring, and then 1.8542 g of 4-PEPA and 5 g of m-cresol were added. The solid content of the solution was adjusted to 29 wt %, and the reaction was continued for 4 h. Then, under nitrogen protection, the reaction system was heated to 195° C. and reacted for 6 h. After the reaction system was cooled to room temperature, it was poured into ethanol, filtered and washed three times, and dried at 240° C. for 2 h to obtain a thermosetting polyimide resin as shown in formula (x).
[0121]
[0122] Structural characterization:
[0123] The thermosetting polyimide resin prepared in this embodiment has a soluble solid content of 30% in the polar aprotic solvent N-methylpyrrolidone, a minimum melt viscosity of 963 Pa·s, a glass transition temperature of 335° C., an elongation at break of 3.4%, and a 5% thermal weight loss temperature in air of 520° C.
[0124] Figure 1 FT-IR spectrum of the thermosetting polyimide resin prepared in Example 1 of the present invention, with a wave number of 2211 cm -1 The C≡C stretching vibration peak of phenylethynyl is at 1776cm -1 and 1720cm -1 The peaks at 1370 cm-1 are the asymmetric and symmetric stretching vibration peaks of the carbonyl C=O on the imide ring. -1 is the CN stretching vibration peak on the imide ring, indicating that the present invention successfully prepared the thermosetting polyimide resin with the structure described in formula (I).
[0125] Figure 2 This is the DSC curve of the thermosetting polyimide resin prepared in Example 1 of the present invention. The endothermic peak at 200-240°C represents the resin melting endothermic process, and the exothermic peak between 330°C and 430°C is attributed to the exothermic cross-linking reaction of phenylethynylphthalic anhydride end-capping. The melting peak and the exothermic peak temperature range >100°C, indicating that this type of resin has a wide processing window.
[0126] Figure 3 This is the rheological curve of the thermosetting polyimide resin prepared in Example 1 of the present invention. The temperature is about 330° C. and the minimum melt viscosity is 3 Pa·s. The process performance is good and it is suitable for molding and autoclave processes.
[0127] Figure 4 DMA curve of the thermosetting polyimide resin prepared in Example 1 of the present invention, 385° C. corresponds to the glass transition temperature of the cured resin.
[0128] Figure 5 3 is a TGA curve of the cured thermosetting polyimide resin prepared in Example 1 of the present invention. It can be seen that the thermal decomposition temperature of the cured polyimide resin at 5 wt % is as high as 573° C., and the cured polyimide resin has excellent heat resistance.
[0129] Figure 6 3 is a diagram of the mechanical properties of the thermosetting polyimide resin prepared in Example 1 of the present invention. It can be seen that the elongation at break of the cured polyimide resin is 2.5%, which means that the cured polyimide resin has relatively good mechanical properties.
[0130] Figure 7This is a solubility performance diagram of the thermosetting polyimide resin prepared in Example 1 of the present invention in NMP, DMAC, DMF, and 1,4-dioxane, and the solid content thereof all reaches 30%, indicating that the thermosetting polyimide resin of the present invention has the characteristic of high solubility and is a soluble thermosetting polyimide resin.
[0131] Performance Discussion:
[0132] Table 1 lists the solubility, rheological properties, thermal weight loss temperature and elongation at break of typical embodiments 3-5 of the present invention and the reported thermosetting polyimide synthesized from fluorene dianhydride (BPAF) and flexible diamine (4,4'-ODA). It can be seen from the table that the solubility, rheological properties, thermal weight loss temperature and elongation at break of embodiments 3-5 are better than those of BPAF-4,4'-ODA (n=3) polyimide resin in the literature (reference: Polymer 2023,281,126086).
[0133] Table 1. Solubility, rheology, thermal weight loss, and elongation at break data of polyimide resin
[0134]
[0135] It can be seen from the above experimental results that the thermosetting polyimide resin of the present invention has the characteristics of high solubility and low viscosity and good processability; and the cured thermosetting polyimide resin of the present invention has both good high temperature resistance and high toughness.
[0136] In addition, the present invention also refers to the aforementioned embodiments and conducts experiments with other raw materials, process operations, and process conditions described in this specification, and obtains relatively ideal results.
[0137] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0138] The use of headings and sections in this disclosure is not meant to limit the disclosure; each section may apply to any aspect, embodiment, or feature of the disclosure.
[0139] Throughout this disclosure, where a composition is described as having, containing, or comprising particular components, or where a process is described as having, containing, or comprising particular process steps, it is contemplated that the compositions taught by the present invention also consist essentially of, or consist of, the recited components, and that the processes taught by the present invention also consist essentially of, or consist of, the recited process steps.
[0140] It should be understood that the order of the various steps or the order in which a particular action is performed is not very important, as long as the teachings of the present invention remain operable. In addition, two or more steps or actions may be performed simultaneously.
[0141] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.
Claims
1. A thermosetting polyimide resin, characterized in that: The thermosetting polyimide resin has a structure as shown in formula (I): Wherein, n is any positive number from 1 to 10, and each Ar is independently a structure represented by any of the following formulae: R is a structure represented by any of the following formulae: The dotted line represents the insertion position of the amino group.
2. The thermosetting polyimide resin according to claim 1, characterized in that: The dissolved solid content of the thermosetting polyimide resin in the polar aprotic solvent is greater than 30%; And / or, the minimum melt viscosity of the thermosetting polyimide resin is 3 to 1254 Pa·s; And / or, the cured product of the thermosetting polyimide resin has a glass transition temperature of 335 to 425° C.; And / or, the cured product of the thermosetting polyimide resin has a 5% thermal weight loss temperature in air higher than 520° C. and an elongation at break higher than 2%.
3. The method for preparing a thermosetting polyimide resin according to any one of claims 1 to 2, characterized in that: include: S1, under a protective atmosphere, mixing an aromatic diamine monomer, an ether-containing fluorene dianhydride monomer and an organic solvent, and reacting at 95-105° C. for 6-8 hours; S2, adding a capping agent to the mixed reaction system obtained in step S1, and continuing the reaction at 95-105° C. for 2-4 hours; S3, heating the reaction mixture obtained in step S2 to 195-205° C. and continuing the reaction for 4-6 hours; S4, mixing the reaction mixture obtained in step S3 with a cleaning agent to precipitate a solid, and washing and drying the obtained solid to obtain a thermosetting polyimide resin.
4. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S1, the ether-containing fluorene anhydride monomer has a structure as shown in formula (II):
5. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S1, the aromatic diamine monomer is any one of 2,2'-bis(trifluoromethyl)-4,4'-diaminophenyl ether, 4,4'-[1,4-phenylbis(oxy)]bis[3-(trifluoromethyl)aniline], 1,3-phenylenediamine, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 9,9-bis(4-aminophenyl)fluorene, [1,1':3',1"-terphenyl]-4,4"-diamine, [1,1':3',1"-terphenyl]-3,3"-diamine and [1,1':4',1"-terphenyl]-3,3"-diamine, or a combination of two or more thereof.
6. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S1, the molar ratio of the ether-containing fluorene anhydride monomer, the aromatic diamine monomer and the end-capping agent is n:(n+1):2, wherein n>0.
7. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S1, the organic solvent is any one of m-cresol and sulfolane or a combination of two or more thereof.
8. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S2, the end-capping agent is any one of 4-phenylethynylphthalic anhydride, ethynylphthalic anhydride and norbornene dicarboxylic anhydride; And / or, in step S2, after adding the end-capping agent to the mixed reaction system obtained in step S1, the solid content in the obtained mixed solution is controlled to 20wt% to 40wt%, and the reaction is continued for 2 to 4h.
9. The method for preparing a thermosetting polyimide resin according to claim 3, characterized in that: In step S4, the cleaning agent is one or more of methanol, ethanol or deionized water; And / or, in step S4, the drying temperature is 220-240°C.
10. A polyimide resin-based composite material, characterized in that: The invention comprises the thermosetting polyimide resin according to any one of claims 1 to 2.
Citation Information
Patent Citations
Polyimide gas separation membrane as well as preparation method and applications thereof
CN104829853A
Application of thermosetting polyimide in preparation of high-temperature-resistant resin-based composite material
CN114369243A
Thermoplastic polyimide and application thereof in temporary bonding technology
CN116554473A
Aromatic polyimide resin precursor and aromatic polyimide resin
JP2006206825A
Cited By
Soluble polyimide resin as well as preparation method and application thereof
CN120463935A
High-temperature-resistant low-dielectric thermosetting polyimide resin prepolymer as well as preparation method and application thereof
CN121699147A