Preparation process of low-viscosity methyl silicone oil

By using S2O2-8/SnO2-CeO2 solid super acid catalyst and carboxymethylcellulose-montmorillonite composite adsorbent, the problems of large catalyst dosage and difficult removal of impurities in the preparation of low-viscosity methyl silicone oil are solved, and the product yield is improved. and purity, reducing contamination.

CN118755089AInactive Publication Date: 2024-10-11JIANGXI KERUI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411067934.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing low-viscosity methyl silicone oil preparation process, the amount of acid catalyst is large, the product yield is low, and impurities are difficult to remove, affecting product purity and equipment safety.

Method used

Using S2O2-8/SnO2-CeO2 solid super acid catalyst and carboxymethyl cellulose-montmorillonite composite adsorbent, the catalyst is prepared through plasma etching and roasting to improve catalytic activity and purification effect and reduce impurity residues.

Benefits of technology

It improves the yield and purity of low-viscosity methyl silicone oil, reduces catalyst pollution and equipment corrosion, and ensures product quality and safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of silicone oil preparation, in particular to a preparation process of low-viscosity methyl silicone oil. The invention relates to a preparation process of low-viscosity methyl silicone oil. The preparation process comprises the following steps: preparation of a catalyst precursor, preparation of an S2O2-8 / SnO2-CeO2 solid superacid catalyst, preparation of a carboxymethyl chitosan-montmorillonite composite adsorbent and synthesis of the low-viscosity methyl silicone oil. In the synthesis process of the low-viscosity methyl silicone oil, the ring-opening polymerization reaction is carried out by utilizing the catalytic action of the S2O2-8 / SnO2-CeO2 solid superacid catalyst, so that the reaction can be promoted, the yield of the low-viscosity methyl silicone oil product is improved, and the formation of low-viscosity silicone oil is promoted; the carboxymethyl cellulose-montmorillonite composite adsorbent is used for adsorbing and purifying the solution after the ring-opening polymerization reaction and before reduced pressure distillation, so that impurities in the low-viscosity methyl silicone oil can be effectively removed, and the quality of the low-viscosity methyl silicone oil is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silicone oil preparation, and more specifically, to a preparation process of low-viscosity methyl silicone oil. Background Art

[0002] Low viscosity methyl silicone oil, generally refers to a kinematic viscosity below 50mm 2 / s methyl silicone oil has good compatibility with white oil, ethanol and common oils and has a light skin feel. It can be used in oil-in-water, water-in-oil and full-oil systems. It is an important functional main and auxiliary material in the field of modern daily chemical products and is suitable for coatings, personal care products and some industrial cleaning agents.

[0003] The existing low-viscosity methyl silicone oil preparation process usually causes the raw materials to undergo a ring-opening polymerization reaction under the action of a catalyst to generate low-viscosity methyl silicone oil. The catalytic methods are mainly divided into acid catalysis and base catalysis. The acid catalysis method usually uses concentrated sulfuric acid, trifluoromethylsulfonic acid or a solid acid catalyst as a catalyst, while the base catalysis method may use potassium hydroxide, tetramethylammonium hydroxide, etc. as a catalyst. Among them, the acid catalyst used in the acid catalysis method has high catalytic activity, but its dosage is large, the product yield is low, and the post-processing is relatively cumbersome. For example, concentrated sulfuric acid and trifluoromethylsulfonic acid need to be neutralized after the reaction. The salts and residual acid and alkali impurities after neutralization are not easy to remove and are easily left in the low-viscosity methyl silicone oil. The purity and quality of the low-viscosity methyl silicone oil cannot be well guaranteed, and there are also problems such as high corrosion and high pollution to the equipment during actual use.

[0004] Furthermore, as a highly pure polydimethylsiloxane liquid, the production process of low-viscosity methyl silicone oil usually requires extremely high purity standards. If impurities such as dust, metal debris, incompletely reacted raw material particles or other insoluble substances are added during the production and preparation process, these impurities may interfere with the interaction between methyl silicone oil molecules, thereby affecting the rheological properties of low-viscosity methyl silicone oil, changing the kinematic viscosity of low-viscosity methyl silicone oil, and further affecting the use effect of low-viscosity methyl silicone oil. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a preparation process of low-viscosity methyl silicone oil.

[0006] A preparation process of low-viscosity methyl silicone oil comprises the following steps:

[0007] S1: Preparation of catalyst precursor, dissolving SnCl4·5H2O and Ce(NO3)3·6H2O in deionized water to obtain a mixed aqueous solution, adding a surfactant, wherein the mass ratio of the mixed aqueous solution to the surfactant is (450-500):1, adding ammonia water dropwise while stirring to make the pH of the mixed aqueous solution = 9-10, continuing stirring to gradually form a precipitate, and performing static aging, centrifugal separation, filtering, taking the precipitate, washing, drying and grinding to obtain a catalyst precursor;

[0008] S2: S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation, the catalyst precursor is completely immersed in (NH4)2S2O8 solution, filtered, dried, plasma etched and calcined to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst;

[0009] S3: Preparation of carboxymethyl chitosan-montmorillonite composite adsorbent, 18-25 parts by weight of carboxymethyl cellulose, 80-150 parts by weight of deionized water, 4-12 parts by weight of 10% ammonium persulfate solution, 13-20 parts by weight of acrylic acid monomer with a neutralization degree of 40-60% and 10-15 parts by weight of acrylamide are stirred and mixed to obtain a mixture, 20-45 parts by weight of montmorillonite and 60-90 parts by weight of deionized water are mixed to obtain a montmorillonite suspension, the mixture, 2-14 parts by weight of N,N-methylenebisacrylamide and 1-8 parts by weight of sodium bisulfite are added to the montmorillonite suspension, and the mixture is stirred, filtered, washed and dried to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent;

[0010] S4: Synthesis of low viscosity methyl silicone oil, dimethyl carbonate, hexamethyldisiloxane and S2O 2-8 / SnO2-CeO2 solid superacid catalyst is stirred and mixed in proportion, and the temperature is raised for reaction for a period of time. After the reaction is completed, S2O 2-8 / SnO2-CeO2 solid superacid catalyst was taken out and cleaned for use, and S2O 2-8 / SnO2-CeO2 solid superacid catalyst, the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane, decamethyltetrasiloxane and dimethyl carbonate are stirred and mixed according to a certain proportion, heated and dehydrated for a period of time, and the above-mentioned washed S2O 2-8 / SnO2-CeO2 solid superacid catalyst continues to dehydrate for a period of time, then undergoes polymerization reaction, heat preservation, and takes out S2O 2-8 / SnO2-CeO2 solid superacid catalyst, carboxymethyl chitosan-montmorillonite composite adsorbent is added to the remaining liquid for adsorption purification treatment, and then low-viscosity methyl silicone oil is obtained through reduced pressure distillation, cooling and filtration.

[0011] Furthermore, step S1 of preparing a catalyst precursor specifically comprises the following steps:

[0012] S1.1: Dissolve 10 to 30 parts by weight of SnCl4·5H2O and 12 to 26 parts by weight of Ce(NO3)3·6H2O in 100 to 200 parts by weight of deionized water to obtain a mixed aqueous solution, add a surfactant to the mixed aqueous solution, wherein the mass ratio of the mixed aqueous solution to the surfactant is (450 to 500):1, add ammonia water dropwise while stirring to make the pH of the mixed aqueous solution = 9 to 10, continue stirring for 30 to 50 minutes, thereby gradually forming a precipitate;

[0013] S1.2: After stirring, adjust the temperature to 0-5°C, let it stand for 20-24 hours, then centrifuge, filter and precipitate, wash the precipitate with a 5% ammonium acetate aqueous solution to a pH of 6.5-7, and then wash it 1-2 times with a 70% alcohol solution by volume. Dry the washed precipitate in a vacuum at 100-120°C for 4-6 hours, then grind the dried precipitate through a 60-80 mesh sieve to obtain a catalyst precursor.

[0014] Furthermore, the surfactant is sodium dodecylbenzene sulfonate.

[0015] Furthermore, in step S1.1, the volume concentration of the ammonia water is 15-25%.

[0016] Furthermore, in step S1.1, the operation speed of adding ammonia water dropwise while stirring is: the stirring speed is 200-400 r / min, and the dropping speed is 20-40 drops / min.

[0017] Further, step S2S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation, specifically comprising the following steps:

[0018] S2.1: The catalyst precursor is completely immersed in a (NH4)2S2O8 solution with a concentration of 1.0 mol / L for 2 to 3 hours, filtered, and vacuum dried at 100 to 110°C for 30 to 50 minutes;

[0019] S2.2: After drying, the catalyst precursor is placed in a plasma etcher for plasma etching;

[0020] S2.3: After etching, the etched catalyst precursor is placed in a muffle furnace and calcined at 500-600°C for 3-4 hours to obtain a S2O2-8 / SnO2-CeO2 solid superacid catalyst.

[0021] Furthermore, in step S2.2, the radio frequency power of the plasma etcher is 100 to 140 W, the argon gas flow rate is 0.3 to 0.6 L / min, and the time is 20 to 30 min.

[0022] Furthermore, step S3 of preparing a carboxymethyl cellulose-montmorillonite composite adsorbent specifically comprises the following steps:

[0023] S3.1: 18 to 25 parts by weight of carboxymethyl cellulose are dissolved in 80 to 150 parts by weight of deionized water, and the mixture is stirred at 50 to 60° C. Subsequently, 4 to 12 parts by weight of a 10% ammonium persulfate solution are added, and the mixture is stirred for 10 to 15 minutes. Then, 13 to 20 parts by weight of an acrylic acid monomer having a neutralization degree of 40 to 60% and 10 to 15 parts by weight of acrylamide are added, and the mixture is stirred for 30 to 50 minutes to obtain a mixture;

[0024] S3.2: adding 20 to 45 parts by weight of montmorillonite to 60 to 90 parts by weight of deionized water, and ultrasonically dispersing for 30 to 45 minutes to obtain a montmorillonite suspension;

[0025] S3.3: Add 2 to 14 parts by weight of N,N-methylenebisacrylamide and 1 to 8 parts by weight of sodium bisulfite to the montmorillonite suspension of step S3.2, stir for 20 to 40 minutes, heat to 60 to 72°C, add the mixture of step S3.1, stir for 1 to 2 hours, and then filter, wash and dry to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent.

[0026] Further, step S4 is the synthesis of low-viscosity methyl silicone oil, which specifically comprises the following steps:

[0027] S4.1: Add dimethyl carbonate and hexamethyldisiloxane into the reactor, the volume ratio of dimethyl carbonate to hexamethyldisiloxane is 1:(1.5-2), stir and mix, then add S2O 2-8 / SnO2-CeO2 solid superacid catalyst, heat to 50-60℃ and react for 3-4h;

[0028] S4.2: After the reaction is completed, remove S2O 2-8 / SnO2-CeO2 solid super acid catalyst, wash the S2O2-8 / SnO2-CeO2 solid super acid catalyst and set it aside, and the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane;

[0029] S4.3: Add decamethyltetrasiloxane and dimethyl carbonate in a volume ratio of 4:(2-3) into the reaction kettle, stir evenly, heat to 60-90°C and dehydrate for 40-60 minutes, then wash the S2O 2-8 / SnO2-CeO2 solid superacid catalyst is added to the reactor and dehydration is continued for 10 to 15 minutes;

[0030] S4.4: After dehydration, heat to 120-130℃ for polymerization for 2-3h, then heat to 150-170℃ for 1-2h. After heat preservation, remove S2O 2-8 / SnO2-CeO2 solid superacid catalyst is taken out, and after the liquid in the reactor is cooled to 32-45°C, carboxymethyl chitosan-montmorillonite composite adsorbent is added, and the mass ratio of carboxymethyl chitosan-montmorillonite composite adsorbent to the liquid in the reactor is (3-9):100, ultrasonic dispersion is performed for 10-20 minutes, and then standing for 40-60 minutes, and the carboxymethyl chitosan-montmorillonite composite adsorbent in the reactor is filtered out;

[0031] S4.5: Then, the remaining filtrate in the reactor is heated to 200-220°C, and low-boiling substances are removed under 2.4-2.7 kPa until no low-boiling substances drip out. After the removal of low-boiling substances, the temperature is lowered to 120-140°C, and the bottom valve of the reactor is opened. Dried compressed air is bubbled into the reactor for 1-3 hours, and then the temperature is naturally lowered to 30-35°C. After filtration, low-viscosity methyl silicone oil is obtained.

[0032] Further, in step S4.1, the sum of the weights of dimethyl carbonate and hexamethyldisiloxane and S2O 2-8 The weight ratio of / SnO2-CeO2 solid super acid catalyst is 100:(5~12).

[0033] The present invention has the following advantages:

[0034] 1. In the present invention, plasma etching is performed on the catalyst precursor to increase S2O 2-8 / SnO2-CeO2 solid superacid catalyst, reduce the pore collapse caused by high temperature calcination, reduce the pore size, and thus help to increase the S2O 2-8 / SnO2-CeO2 solid strong acid catalyst catalytic activity, improve the synthesis yield of low viscosity silicone oil.

[0035] 2. In the present invention, in the process of synthesizing low-viscosity methyl silicone oil, S2O 2-8 / SnO2-CeO2 solid superacid catalyst can not only promote the reaction and increase the yield of low-viscosity methyl silicone oil, but also effectively control the kinematic viscosity of methyl silicone oil and promote the formation of low-viscosity methyl silicone oil. 2-8 / SnO2-CeO2 solid superacid catalyst is easy to separate and can be reused with little pollution.

[0036] 3. In the present invention, the residual filtrate in the reactor is subjected to adsorption and purification treatment by using a carboxymethyl cellulose-montmorillonite composite adsorbent, which can effectively remove impurities therein, thereby facilitating the improvement of the quality of the low-viscosity methyl silicone oil and ensuring the kinematic viscosity of the low-viscosity methyl silicone oil. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0038] Example 1

[0039] A preparation process of low-viscosity methyl silicone oil specifically comprises the following steps:

[0040] S1: Catalyst precursor preparation,

[0041] S1.1: 30 parts by weight of SnCl4·5H2O and 26 parts by weight of Ce(NO3)3·6H2O are dissolved in 140 parts by weight of deionized water to obtain a mixed aqueous solution, sodium dodecylbenzene sulfonate is added to the mixed aqueous solution, wherein the mass ratio of the mixed aqueous solution to the sodium dodecylbenzene sulfonate is 500:1, and ammonia water with a volume concentration of 25% is added dropwise while stirring, the stirring speed is 400 r / min, and the dropping speed is 40 drops / min, so that the pH of the mixed aqueous solution is 9, and stirring is continued for 50 minutes, thereby gradually forming a precipitate;

[0042] S1.2: After the stirring is completed, the temperature is adjusted to 5°C, and the mixture is allowed to stand for 24 hours. Subsequently, the mixture is centrifuged, filtered, and precipitated. The precipitate is washed with a 5% ammonium acetate aqueous solution to a pH of 7, and then washed twice with a 70% alcohol solution. The washed precipitate is vacuum dried at 120°C for 6 hours. Then, the dried precipitate is ground through an 80-mesh sieve to obtain a catalyst precursor.

[0043] S2: S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation,

[0044] S2.1: The catalyst precursor was completely immersed in a (NH4)2S2O8 solution with a concentration of 1.0 mol / L for 3 h, filtered, and vacuum dried at 110 °C for 50 min;

[0045] S2.2: After drying, the catalyst precursor is placed in a plasma etcher for plasma etching. The RF power of the plasma etcher is 140 W, the argon gas flow rate is 0.6 L / min, and the time is 30 min.

[0046] S2.3: After etching, the etched catalyst precursor is placed in a muffle furnace and calcined at 600 °C for 4 h to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst;

[0047] S3: Preparation of carboxymethyl cellulose-montmorillonite composite adsorbent,

[0048] S3.1: 25 parts by weight of carboxymethyl cellulose are dissolved in 150 parts by weight of deionized water, and the mixture is stirred at 60° C. Subsequently, 12 parts by weight of a 10% ammonium persulfate solution is added, and the mixture is stirred for 15 minutes. Then, 20 parts by weight of an acrylic acid monomer having a neutralization degree of 60% and 15 parts by weight of acrylamide are added, and the mixture is stirred for 50 minutes to obtain a mixture;

[0049] S3.2: adding 45 parts by weight of montmorillonite to 90 parts by weight of deionized water, and ultrasonically dispersing for 45 minutes to obtain a montmorillonite suspension;

[0050] S3.3: 14 parts by weight of N,N-methylenebisacrylamide and 8 parts by weight of sodium bisulfite are added to the montmorillonite suspension of step S3.2, stirred for 40 minutes, heated to 72°C, and then added to the mixture of step S3.1, stirred for 2 hours, and then filtered, washed and dried to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent;

[0051] S4: low viscosity methyl silicone oil synthesis,

[0052] S4.1: Add dimethyl carbonate and hexamethyldisiloxane into the reactor in a volume ratio of 1:2, stir and mix, then add S2O 2-8 / SnO2-CeO2 solid superacid catalyst, the sum of the weight of dimethyl carbonate and hexamethyldisiloxane and S2O 2-8 / SnO2-CeO2 solid superacid catalyst weight ratio is 100:12, the temperature is raised to 60℃ and the reaction is carried out for 4h;

[0053] S4.2: After the reaction is completed, remove S2O 2-8 / SnO2-CeO2 solid super acid catalyst, wash the S2O2-8 / SnO2-CeO2 solid super acid catalyst and set it aside, and the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane;

[0054] S4.3: Add decamethyltetrasiloxane and dimethyl carbonate into the reaction kettle in a volume ratio of 4:3, stir evenly, heat to 90°C and dehydrate for 60 minutes, then wash the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was added to the reactor and dehydration was continued for 15 min;

[0055] S4.4: After dehydration, the temperature was raised to 130℃ for polymerization for 3h, then the temperature was raised to 170℃ for 2h. After the insulation, the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was taken out, and after the liquid in the reactor was cooled to 45°C, carboxymethyl chitosan-montmorillonite composite adsorbent was added, and the mass ratio of carboxymethyl chitosan-montmorillonite composite adsorbent to the liquid in the reactor was 9:100, ultrasonic dispersion was performed for 20 minutes, and then the mixture was allowed to stand for 60 minutes, and the carboxymethyl chitosan-montmorillonite composite adsorbent in the reactor was filtered out;

[0056] S4.5: Then, the remaining filtrate in the reactor was heated to 220°C, and low-boiling substances were removed under 2.7 kPa until no low-boiling substances dripped out. After the removal of low-boiling substances, the temperature was lowered to 140°C, and the bottom valve of the reactor was opened. The dried compressed air was bubbled into the reactor for 3 hours, and then the temperature was naturally lowered to 35°C. After filtration, low-viscosity methyl silicone oil was obtained.

[0057] Example 2

[0058] A preparation process of low-viscosity methyl silicone oil specifically comprises the following steps:

[0059] S1: Catalyst precursor preparation,

[0060] S1.1: 30 parts by weight of SnCl4·5H2O and 26 parts by weight of Ce(NO3)3·6H2O are dissolved in 140 parts by weight of deionized water to obtain a mixed aqueous solution, sodium dodecylbenzene sulfonate is added to the mixed aqueous solution, wherein the mass ratio of the mixed aqueous solution to the sodium dodecylbenzene sulfonate is 500:1, and ammonia water with a volume concentration of 25% is added dropwise while stirring, the stirring speed is 200 r / min, and the dropping speed is 20 drops / min, so that the pH of the mixed aqueous solution is 10, and stirring is continued for 30 minutes, thereby gradually forming a precipitate;

[0061] S1.2: After the stirring is completed, the temperature is adjusted to 0°C, and the mixture is allowed to stand for 20 hours. Subsequently, the mixture is centrifuged, filtered, and precipitated. The precipitate is washed with a 5% ammonium acetate aqueous solution to a pH of 6.5, and then washed twice with a 70% alcohol solution. The washed precipitate is vacuum dried at 100°C for 4 hours. Subsequently, the dried precipitate is ground through an 80-mesh sieve to obtain a catalyst precursor.

[0062] S2: S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation,

[0063] S2.1: The catalyst precursor is completely immersed in a (NH4)2S2O8 solution with a concentration of 1.0 mol / L for 2 h, filtered, and vacuum dried at 100 °C for 30 min;

[0064] S2.2: After drying, the catalyst precursor is placed in a plasma etcher for plasma etching. The RF power of the plasma etcher is 140 W, the argon gas flow rate is 0.6 L / min, and the time is 20 min.

[0065] S2.3: After etching, the etched catalyst precursor is placed in a muffle furnace and calcined at 500 °C for 3 h to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst;

[0066] S3: Preparation of carboxymethyl cellulose-montmorillonite composite adsorbent,

[0067] S3.1: 25 parts by weight of carboxymethyl cellulose are dissolved in 150 parts by weight of deionized water, and the mixture is stirred at 50° C. Subsequently, 12 parts by weight of a 10% ammonium persulfate solution is added, and the mixture is stirred for 10 minutes. Then, 20 parts by weight of an acrylic acid monomer having a neutralization degree of 60% and 15 parts by weight of acrylamide are added, and the mixture is stirred for 50 minutes to obtain a mixture;

[0068] S3.2: adding 45 parts by weight of montmorillonite to 90 parts by weight of deionized water, and ultrasonically dispersing for 30 minutes to obtain a montmorillonite suspension;

[0069] S3.3: 14 parts by weight of N,N-methylenebisacrylamide and 8 parts by weight of sodium bisulfite are added to the montmorillonite suspension of step S3.2, stirred for 20 minutes, heated to 60°C, and then added to the mixture of step S3.1, stirred for 1 hour, and then filtered, washed and dried to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent;

[0070] S4: low viscosity methyl silicone oil synthesis,

[0071] S4.1: Add dimethyl carbonate and hexamethyldisiloxane into the reactor in a volume ratio of 1:2, stir and mix, then add S2O 2-8 / SnO2-CeO2 solid superacid catalyst, the sum of the weight of dimethyl carbonate and hexamethyldisiloxane and S2O 2-8 / SnO2-CeO2 solid superacid catalyst weight ratio is 100:12, the temperature is raised to 50℃ and the reaction is carried out for 3h;

[0072] S4.2: After the reaction is completed, remove S2O 2-8 / SnO2-CeO2 solid super acid catalyst, wash the S2O2-8 / SnO2-CeO2 solid super acid catalyst and set it aside, and the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane;

[0073] S4.3: Add decamethyltetrasiloxane and dimethyl carbonate into the reactor in a volume ratio of 4:3, stir evenly, heat to 60°C and dehydrate for 40 minutes, then wash the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was added to the reactor and dehydration was continued for 10 min;

[0074] S4.4: After dehydration, the temperature was raised to 120°C for polymerization for 2 hours, then raised to 150°C for 1 hour. After the insulation was completed, the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was taken out, and after the liquid in the reactor was cooled to 32°C, carboxymethyl chitosan-montmorillonite composite adsorbent was added, and the mass ratio of carboxymethyl chitosan-montmorillonite composite adsorbent to the liquid in the reactor was 9:100. Ultrasonic dispersion was performed for 10 minutes, and then the mixture was allowed to stand for 40 minutes. The carboxymethyl chitosan-montmorillonite composite adsorbent in the reactor was filtered out;

[0075] S4.5: Then, the remaining filtrate in the reactor is heated to 200°C, and low-boiling substances are removed under 2.4 kPa until no low-boiling substances drip out. After the removal of low-boiling substances, the temperature is lowered to 120°C, and the bottom valve of the reactor is opened. Dried compressed air is bubbled into the reactor for 1 hour, and then the temperature is naturally lowered to 30°C. After filtration, low-viscosity methyl silicone oil is obtained.

[0076] Example 3

[0077] A preparation process of low-viscosity methyl silicone oil specifically comprises the following steps:

[0078] S1: Catalyst precursor preparation,

[0079] S1.1: Dissolve 10 parts by weight of SnCl4·5H2O and 12 parts by weight of Ce(NO3)3·6H2O in 100 parts by weight of deionized water to obtain a mixed aqueous solution, add sodium dodecylbenzene sulfonate to the mixed aqueous solution, wherein the mass ratio of the mixed aqueous solution to the sodium dodecylbenzene sulfonate is 450:1, and drip ammonia water with a volume concentration of 25% while stirring, the stirring speed is 400 r / min, and the dripping speed is 40 drops / min, so that the pH of the mixed aqueous solution is 9, and continue stirring for 50 minutes, thereby gradually forming a precipitate;

[0080] S1.2: After the stirring is completed, the temperature is adjusted to 5°C, and the mixture is allowed to stand for 24 hours. Subsequently, the mixture is centrifuged, filtered, and precipitated. The precipitate is washed with a 5% ammonium acetate aqueous solution to a pH of 7, and then washed twice with a 70% alcohol solution. The washed precipitate is vacuum dried at 120°C for 6 hours. Then, the dried precipitate is ground through an 80-mesh sieve to obtain a catalyst precursor.

[0081] S2: S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation,

[0082] S2.1: The catalyst precursor was completely immersed in a (NH4)2S2O8 solution with a concentration of 1.0 mol / L for 3 h, filtered, and vacuum dried at 110 °C for 50 min;

[0083] S2.2: After drying, the catalyst precursor is placed in a plasma etcher for plasma etching. The RF power of the plasma etcher is 140 W, the argon gas flow rate is 0.6 L / min, and the time is 30 min.

[0084] S2.3: After etching, the etched catalyst precursor is placed in a muffle furnace and calcined at 600 °C for 4 h to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst;

[0085] S3: Preparation of carboxymethyl cellulose-montmorillonite composite adsorbent,

[0086] S3.1: 18 parts by weight of carboxymethyl cellulose are dissolved in 80 parts by weight of deionized water, and the mixture is stirred at 60° C. Subsequently, 4 parts by weight of a 10% ammonium persulfate solution is added, and the mixture is stirred for 15 minutes. Then, 13 parts by weight of an acrylic acid monomer having a neutralization degree of 60% and 10 parts by weight of acrylamide are added, and the mixture is stirred for 50 minutes to obtain a mixture;

[0087] S3.2: adding 20 parts by weight of montmorillonite to 60 parts by weight of deionized water, and ultrasonically dispersing for 45 minutes to obtain a montmorillonite suspension;

[0088] S3.3: Add 5 parts by weight of N,N-methylenebisacrylamide and 3 parts by weight of sodium bisulfite to the montmorillonite suspension of step S3.2, stir for 40 minutes, heat to 72°C, add the mixture of step S3.1, stir for 2 hours, and then filter, wash and dry to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent;

[0089] S4: low viscosity methyl silicone oil synthesis,

[0090] S4.1: Add dimethyl carbonate and hexamethyldisiloxane into the reactor, the volume ratio of dimethyl carbonate to hexamethyldisiloxane is 1:1.5, stir and mix, then add S2O 2-8 / SnO2-CeO2 solid superacid catalyst, the sum of the weight of dimethyl carbonate and hexamethyldisiloxane and S2O 2-8 / SnO2-CeO2 solid superacid catalyst weight ratio is 100:5, the temperature is raised to 60℃ and the reaction is carried out for 4h;

[0091] S4.2: After the reaction is completed, remove S2O 2-8 / SnO2-CeO2 solid super acid catalyst, wash the S2O2-8 / SnO2-CeO2 solid super acid catalyst and set it aside, and the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane;

[0092] S4.3: Add decamethyltetrasiloxane and dimethyl carbonate into the reactor in a volume ratio of 2:1, stir evenly, heat to 90°C and dehydrate for 60 minutes, then wash the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was added to the reactor and dehydration was continued for 15 min;

[0093] S4.4: After dehydration, the temperature was raised to 130℃ for polymerization for 3h, then the temperature was raised to 170℃ for 2h. After the insulation, the S2O 2-8 / SnO2-CeO2 solid superacid catalyst was taken out, and after the liquid in the reactor was cooled to 45°C, carboxymethyl chitosan-montmorillonite composite adsorbent was added, and the mass ratio of carboxymethyl chitosan-montmorillonite composite adsorbent to the liquid in the reactor was 3:100. Ultrasonic dispersion was performed for 20 minutes, and then the mixture was allowed to stand for 60 minutes. The carboxymethyl chitosan-montmorillonite composite adsorbent in the reactor was filtered out;

[0094] S4.5: Then, the remaining filtrate in the reactor was heated to 220°C, and low-boiling substances were removed under 2.7 kPa until no low-boiling substances dripped out. After the removal of low-boiling substances, the temperature was lowered to 140°C, and the bottom valve of the reactor was opened. The dried compressed air was bubbled into the reactor for 3 hours, and then the temperature was naturally lowered to 35°C. After filtration, low-viscosity methyl silicone oil was obtained.

[0095] Comparative Example 1

[0096] Compared with Example 1, the difference of Comparative Example 1 is that step S2.2 is removed, and the catalyst precursor dried in step S2.1 is directly placed in a muffle furnace for calcination to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst, and the other steps remain unchanged to prepare low viscosity methyl silicone oil, which is recorded as Comparative Example 1.

[0097] The S2O in Examples 1-3 and Comparative Example 1 was analyzed and calculated using a high-resolution transmission electron microscope. 2-8 / SnO2-CeO2 solid superacid catalyst pore structure parameters, the results are shown in Table 1.

[0098] Table 1:

[0099] Group <![CDATA[Specific surface area (m 2 / g)]]> Pore ​​size (nm) <![CDATA[Pore volume (cm 3 / g)]]> Example 1 124.2 10.1 0.21 Example 2 118.7 13.2 0.27 Example 3 120.5 11.5 0.2 Comparative Example 1 105.3 17.1 0.15

[0100] As shown in Table 1, the S2O in Examples 1-3 2-8 / SnO2-CeO2 solid superacid catalyst, the specific surface area and pore volume are greater than those of S2O in comparative example 1 2-8 / SnO2-CeO2 solid superacid catalyst, and the pore size is smaller than that of S2O 2-8 / SnO2-CeO2 solid superacid catalyst, indicating that after plasma etching, S2O 2-8 The specific surface area and pore volume of the SnO2-CeO2 solid superacid catalyst are increased, while the increase in pore size caused by pore collapse to form mesopores due to high-temperature calcination is reduced.

[0101] Comparative Example 2

[0102] Compared with Example 1, the difference of Comparative Example 2 is that the S2O used in step S4 is 2-8 / SnO2-CeO2 solid super acid catalyst was removed, and the other steps remained unchanged to prepare low viscosity methyl silicone oil, which was recorded as Comparative Example 2.

[0103] Comparative Example 3

[0104] Compared with Example 1, the difference of Comparative Example 3 is that the S2O in step S4.1 and step S4.3 is 2-8 / SnO2-CeO2 solid superacid catalyst is replaced with trifluoromethanesulfonic acid. In step S4.2, after the reaction is completed, sodium bicarbonate is added to the reactor so that the pH of the solution in the reactor is 7. In step S4.3, after the dehydration is completed, sodium bicarbonate is added to the reactor so that the pH of the solution in the reactor is 7. The other steps remain unchanged to prepare low-viscosity methyl silicone oil, which is recorded as Comparative Example 3.

[0105] The yield of the low-viscosity methyl silicone oil of Examples 1-3 and Comparative Examples 1-3 was calculated, wherein the yield calculation formula was: D(%) = m / (m1+m2)*100%, m was the mass of the low-viscosity methyl silicone oil, m1 and m2 were the masses of dimethyl carbonate and hexamethyldisiloxane, respectively; and, in accordance with the standard of GB / T10247-2008, the kinematic viscosity of the low-viscosity methyl silicone oil in Examples 1-3 and Comparative Examples 1-3 was determined, and the results were shown in Table 2.

[0106] Table 2:

[0107] Group Yield (%) <![CDATA[Viscosity (mm 2 / s)]]> Example 1 97.4 9.3 Example 2 96.8 11.7 Example 3 97.1 10.4 Comparative Example 1 92.3 16.5 Comparative Example 2 23.6 358.3 Comparative Example 3 62.4 10.8

[0108] As shown in Table 2, the yields of low-viscosity methyl silicone oils in Examples 1-3 were all higher than 96%, which were better than those in Comparative Examples 1-3. 2-8 / SnO2-CeO2 solid superacid catalyst is used as a synthesis catalyst for low-viscosity methyl silicone oil, which can effectively promote the reaction and improve the yield of low-viscosity methyl silicone oil. In addition, the kinematic viscosity of the low-viscosity methyl silicone oil of Examples 1-3 is small and meets the low viscosity standard.

[0109] Comparative Example 4

[0110] Compared with Example 1, the difference of Comparative Example 4 is that the addition and removal of the carboxymethyl chitosan-montmorillonite composite adsorbent in steps S4.4-S4.5 are removed, and the S2O 2-8 / SnO2-CeO2 and after the cooling is completed, the liquid in the reactor is directly subjected to reduced pressure distillation, and the other steps remain unchanged to prepare low-viscosity methyl silicone oil, which is recorded as Comparative Example 4.

[0111] The mechanical impurity content of the low-viscosity methyl silicone oils of Examples 1-3 and Comparative Example 4 was detected using a mechanical impurity analyzer, and the kinematic viscosity of the low-viscosity methyl silicone oils of Examples 1-3 and Comparative Example 4 was measured in accordance with the standard of GB / T10247-2008. The results are shown in Table 3.

[0112] Table 3:

[0113] Group Mechanical impurity content (%) <![CDATA[Viscosity (mm 2 / s)]]> Example 1 0.0014 9.3 Example 2 0.0019 11.7 Example 3 0.0016 10.4 Comparative Example 4 0.0057 12.6

[0114] As can be seen from Table 3, the mechanical impurity content of the low-viscosity methyl silicone oil in Examples 1-3 is less than that in Comparative Example 4, indicating that the adsorption and purification treatment using the carboxymethyl chitosan-montmorillonite composite adsorbent can effectively remove the impurities therein, thereby helping to improve the quality of the low-viscosity methyl silicone oil and ensure the kinematic viscosity of the low-viscosity methyl silicone oil.

[0115] It should be understood that those skilled in the art can make improvements or changes based on the above description, and all such improvements and changes should fall within the scope of protection of the appended claims of the present invention. Parts not described in detail in this specification belong to the prior art known to those skilled in the art.

Claims

1. A process for preparing low-viscosity methyl silicone oil, characterized in that: The steps include: S1: Preparation of catalyst precursor, dissolving SnCl4·5H2O and Ce(NO3)3·6H2O in deionized water to obtain a mixed aqueous solution, adding a surfactant, wherein the mass ratio of the mixed aqueous solution to the surfactant is (450-500):1, adding ammonia water dropwise while stirring to make the pH of the mixed aqueous solution = 9-10, continuing stirring to gradually form a precipitate, and performing static aging, centrifugal separation, filtering, taking the precipitate, washing, drying and grinding to obtain a catalyst precursor; S2: S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation, the catalyst precursor is completely immersed in (NH4)2S2O8 solution, filtered, dried, plasma etched and calcined to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst; S3: Preparation of carboxymethyl chitosan-montmorillonite composite adsorbent, 18-25 parts by weight of carboxymethyl cellulose, 80-150 parts by weight of deionized water, 4-12 parts by weight of 10% ammonium persulfate solution, 13-20 parts by weight of acrylic acid monomer with a neutralization degree of 40-60% and 10-15 parts by weight of acrylamide are stirred and mixed to obtain a mixture, 20-45 parts by weight of montmorillonite and 60-90 parts by weight of deionized water are mixed to obtain a montmorillonite suspension, the mixture, 2-14 parts by weight of N,N-methylenebisacrylamide and 1-8 parts by weight of sodium bisulfite are added to the montmorillonite suspension, and the mixture is stirred, filtered, washed and dried to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent; S4: Synthesis of low viscosity methyl silicone oil, dimethyl carbonate, hexamethyldisiloxane and S2O 2-8 / SnO2-CeO2 solid superacid catalyst is stirred and mixed in proportion, and the temperature is raised for reaction for a period of time. After the reaction is completed, S2O 2-8 / SnO2-CeO2 solid superacid catalyst was taken out and cleaned for use, and S2O 2-8 / SnO2-CeO2 solid superacid catalyst, the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane, decamethyltetrasiloxane and dimethyl carbonate are stirred and mixed according to a certain proportion, heated and dehydrated for a period of time, and the above-mentioned washed S2O 2-8 / SnO2-CeO2 solid superacid catalyst continues to dehydrate for a period of time, then undergoes polymerization reaction, heat preservation, and takes out S2O 2-8 / SnO2-CeO2 solid superacid catalyst, carboxymethyl chitosan-montmorillonite composite adsorbent is added to the remaining liquid for adsorption purification treatment, and then low-viscosity methyl silicone oil is obtained through reduced pressure distillation, cooling and filtration.

2. A process for preparing low-viscosity methyl silicone oil according to claim 1, characterized in that: Step S1: Preparation of catalyst precursor, specifically comprising the following steps: S1.1: Dissolve 10 to 30 parts by weight of SnCl4·5H2O and 12 to 26 parts by weight of Ce(NO3)3·6H2O in 100 to 200 parts by weight of deionized water to obtain a mixed aqueous solution, add a surfactant to the mixed aqueous solution, wherein the mass ratio of the mixed aqueous solution to the surfactant is (450 to 500):1, add ammonia water dropwise while stirring to make the pH of the mixed aqueous solution = 9 to 10, continue stirring for 30 to 50 minutes, thereby gradually forming a precipitate; S1.2: After stirring, adjust the temperature to 0-5°C, let it stand for 20-24 hours, then centrifuge, filter and precipitate, wash the precipitate with a 5% ammonium acetate aqueous solution to a pH of 6.5-7, and then wash it 1-2 times with a 70% alcohol solution by volume. Dry the washed precipitate in a vacuum at 100-120°C for 4-6 hours, then grind the dried precipitate through a 60-80 mesh sieve to obtain a catalyst precursor.

3. A process for preparing low-viscosity methyl silicone oil according to claim 2, characterized in that: The surfactant is sodium dodecylbenzene sulfonate.

4. A process for preparing low-viscosity methyl silicone oil according to claim 3, characterized in that: In step S1.1, the volume concentration of aqueous ammonia is 15-25%.

5. A process for preparing low-viscosity methyl silicone oil according to claim 4, characterized in that: In step S1.1, the operation speed of adding ammonia water dropwise while stirring is: the stirring speed is 200-400 r / min, and the dropping speed is 20-40 drops / min.

6. A process for preparing low-viscosity methyl silicone oil according to claim 1, characterized in that: step S2S2O 2-8 / SnO2-CeO2 solid superacid catalyst preparation, specifically comprising the following steps: S2.1: The catalyst precursor is completely immersed in a (NH4)2S2O8 solution with a concentration of 1.0 mol / L for 2 to 3 hours, filtered, and vacuum dried at 100 to 110°C for 30 to 50 minutes; S2.2: After drying, the catalyst precursor is placed in a plasma etcher for plasma etching; S2.3: After etching, the etched catalyst precursor is placed in a muffle furnace and calcined at 500-600°C for 3-4h to obtain S2O 2-8 / SnO2-CeO2 solid super acid catalyst.

7. A process for preparing low-viscosity methyl silicone oil according to claim 6, characterized in that: In step S2.2, the radio frequency power of the plasma etcher is 100 to 140 W, the argon gas flow rate is 0.3 to 0.6 L / min, and the time is 20 to 30 min.

8. A process for preparing low-viscosity methyl silicone oil according to claim 1, characterized in that: Step S3: Preparation of carboxymethyl cellulose-montmorillonite composite adsorbent, specifically comprising the following steps: S3.1: 18 to 25 parts by weight of carboxymethyl cellulose are dissolved in 80 to 150 parts by weight of deionized water, and the mixture is stirred at 50 to 60° C. Subsequently, 4 to 12 parts by weight of a 10% ammonium persulfate solution are added, and the mixture is stirred for 10 to 15 minutes. Then, 13 to 20 parts by weight of an acrylic acid monomer having a neutralization degree of 40 to 60% and 10 to 15 parts by weight of acrylamide are added, and the mixture is stirred for 30 to 50 minutes to obtain a mixture; S3.2: adding 20 to 45 parts by weight of montmorillonite to 60 to 90 parts by weight of deionized water, and ultrasonically dispersing for 30 to 45 minutes to obtain a montmorillonite suspension; S3.3: Add 2 to 14 parts by weight of N,N-methylenebisacrylamide and 1 to 8 parts by weight of sodium bisulfite to the montmorillonite suspension of step S3.2, stir for 20 to 40 minutes, heat to 60 to 72°C, add the mixture of step S3.1, stir for 1 to 2 hours, and then filter, wash and dry to obtain a carboxymethyl cellulose-montmorillonite composite adsorbent.

9. A process for preparing low-viscosity methyl silicone oil according to claim 1, characterized in that: Step S4: low viscosity methyl silicone oil synthesis, specifically comprising the following steps: S4.1: Add dimethyl carbonate and hexamethyldisiloxane into the reactor, the volume ratio of dimethyl carbonate to hexamethyldisiloxane is 1:(1.5-2), stir and mix, then add S2O 2-8 / SnO2-CeO2 solid superacid catalyst, heat to 50-60℃ and react for 3-4h; S4.2: After the reaction is completed, remove S2O 2-8 / SnO2-CeO2 solid superacid catalyst for S2O 2-8 / SnO2-CeO2 solid superacid catalyst is washed and set aside, and the remaining solution is decolorized and filtered to obtain decamethyltetrasiloxane; S4.3: Add decamethyltetrasiloxane and dimethyl carbonate in a volume ratio of 4:(2-3) into the reaction kettle, stir evenly, heat to 60-90°C and dehydrate for 40-60 minutes, then wash the S2O 2-8 / SnO2-CeO2 solid superacid catalyst is added to the reactor and dehydration is continued for 10 to 15 minutes; S4.4: After dehydration, heat to 120-130℃ for polymerization for 2-3h, then heat to 150-170℃ for 1-2h. After heat preservation, remove S2O 2-8 / SnO2-CeO2 solid superacid catalyst is taken out, and after the liquid in the reactor is cooled to 32-45°C, carboxymethyl chitosan-montmorillonite composite adsorbent is added, and the mass ratio of carboxymethyl chitosan-montmorillonite composite adsorbent to the liquid in the reactor is (3-9):100, ultrasonic dispersion is performed for 10-20 minutes, and then standing for 40-60 minutes, and the carboxymethyl chitosan-montmorillonite composite adsorbent in the reactor is filtered out; S4.5: Then, the remaining filtrate in the reactor is heated to 200-220°C, and low-boiling substances are removed under 2.4-2.7 kPa until no low-boiling substances drip out. After the removal of low-boiling substances, the temperature is lowered to 120-140°C, and the bottom valve of the reactor is opened. Dried compressed air is bubbled into the reactor for 1-3 hours, and then the temperature is naturally lowered to 30-35°C. After filtration, low-viscosity methyl silicone oil is obtained.

10. A process for preparing low-viscosity methyl silicone oil according to claim 9, characterized in that: In step S4.1, the sum of the weights of dimethyl carbonate and hexamethyldisiloxane and S2O 2-8 The weight ratio of / SnO2-CeO2 solid super acid catalyst is 100:(5~12).