High-temperature-resistant room-temperature-cured silicone rubber and preparation method thereof
By introducing ferrocene silazane cross-linking agent into silicone rubber, the problems of thermal degradation and oxidation of traditional silicone rubber at high temperatures are solved, significantly improving its performance and stability in high temperature and oxidizing environments, and extending the service life. longevity and reduced material preparation complexity.
Patent Information
- Application Number
- CN202411083281.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Traditional silicone rubber has thermal degradation and oxidation problems under high temperature conditions, resulting in a decline in material performance. The effect of existing antioxidants is unstable and it is difficult to resist high temperature oxidative stress for a long time.
Develop a ferrocene silazane cross-linking agent by synthesizing polylithiated ferrocene lithium salt under nitrogen protection, reacting with hexamethylcyclotrisiloxane and 12-4 crown ether, and adding ammonia gas. Cross-linking to form a cross-linking agent with silicon-nitrogen bonds, used to prepare high-temperature-resistant, room-temperature curing silicone rubber.
Significantly improves the performance and stability of silicone rubber in high temperature and oxidizing environments, reduces thermal degradation and oxidation reactions, extends the service life of the material, and achieves excellent high temperature resistance without adding additional antioxidants .
Smart Images

Figure CN118755091A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicone rubber, and in particular to a high temperature resistant room temperature curing silicone rubber and a preparation method thereof. Background Art
[0002] Silicone rubber has become the material of choice for many high-temperature applications due to its excellent high-temperature resistance, especially in the fields of electronics, construction, and mold manufacturing. In particular, two-component room temperature vulcanized silicone rubber (RTV-2) is widely used because of its easy operation and moderate curing speed. This type of silicone rubber usually relies on the participation of catalysts and trace amounts of water to crosslink and vulcanize to form the final elastomeric structure. In recent years, with the development of materials science, the introduction of new chemical bond structures, such as silicon-nitrogen bonds, through molecular design to improve the stability and service life of materials under extreme conditions has become a research hotspot.
[0003] Although two-component room temperature vulcanized silicone rubber has many advantages, it still has obvious limitations in high temperature applications. First, after the traditional silicone rubber is vulcanized under the action of catalyst and moisture, the residual crosslinking agent and its byproducts will accelerate the thermal degradation of the silicone rubber main chain under high temperature conditions. In addition, the uncrosslinked hydroxyl groups in the silicone rubber and the adsorbed moisture will also cause structural instability at high temperatures, thus affecting the overall thermal stability of the material. Although the introduction of silicon nitrogen bonds can partially eliminate the hydroxyl groups in the silicone rubber system and reduce thermal degradation, the application of this strategy in air atmosphere has been greatly challenged. Due to the participation of oxygen, silicone rubber is prone to thermal oxidation crosslinking, thereby reducing the performance of the material. Existing solutions include adding antioxidants, but the effects of these additives are often unstable and it is difficult to resist oxidative stress at high temperatures for a long time. In addition, although the introduction of ferrocene has enhanced the antioxidant properties, its role and optimal ratio in the silicon nitrogen structure have not been fully studied, and the existing technology has not effectively solved these thermal stability problems at high temperatures.
[0004] In this context, the main task of the present invention is to develop a new type of heat-resistant room temperature vulcanized silicone rubber crosslinker that can exhibit excellent high temperature resistance in air without relying on added antioxidants. In particular, the present invention aims to solve the problem of thermal stability of silicone rubber in high temperature applications, and through an innovative crosslinking strategy, significantly improve the performance and stability of the material in a continuous high temperature and oxidative environment. In addition, this new crosslinker will allow silicone rubber to replace current materials in a wider range of industrial applications, especially in applications that require extremely high heat resistance. By solving this technical challenge, the present invention will drive silicone rubber technology forward to meet the needs of more high-performance applications. Summary of the invention
[0005] In order to achieve the above-mentioned purpose of the invention and to solve the above-mentioned technical problems, the present invention provides a ferrocenylsilazane (FSCA) crosslinking agent, and the specific scheme is as follows:
[0006] The cross-linking agent is prepared by the following steps:
[0007] A1: Under nitrogen protection, ferrocene and n-hexane are mixed and stirred until completely dissolved, a n-hexane solution of butyl lithium and tetramethylethylenediamine are added to the above solution, the reaction mixture is heated to n-hexane reflux, and the reaction is continuously stirred, and then the upper solution is filtered and removed, the precipitate is washed with n-hexane for 3 times, and the obtained precipitate is recrystallized with tetrahydrofuran to obtain a polylithiated ferrocene lithium salt;
[0008] A2: adding tetrahydrofuran to completely dissolve the lithium ferrocenium salt obtained in step A1 under nitrogen protection, adding hexamethylcyclotrisiloxane and 12-4 crown ether to the solution, reacting at room temperature, then dropping the reaction solution into tetrahydrofuran containing dimethyldichlorosilane, and stirring at room temperature;
[0009] A3 removes unreacted dimethyldichlorosilane and solvent under vacuum conditions, and extracts the reaction product with toluene to obtain a polymer containing silicon-chloride terminal groups;
[0010] A4: passing ammonia gas into the toluene solution obtained in step A3 at room temperature until no obvious ammonia gas absorption occurs, and then increasing the temperature and continuing to pass ammonia gas, thereby obtaining a ferrocenylsilazane crosslinking agent.
[0011] Preferably, the molar ratio of ferrocene to butyl lithium is 1:5-1:15.
[0012] Preferably, the preparation method of the cross-linking agent corresponding to each 1.86g of ferrocene is:
[0013] B1 Under nitrogen protection, 1.86 g, 0.01 mol of ferrocene and 20 ml of n-hexane were mixed and stirred until completely dissolved, 62.5 ml of n-hexane solution containing 0.1 mol of butyl lithium and 11.2 ml of tetramethylethylenediamine were added to the above solution, the reaction mixture was heated to n-hexane reflux, and the reaction was stirred for 10 hours, then the upper solution was filtered and removed, the precipitate was washed with 40 ml of n-hexane, and the obtained precipitate was recrystallized using tetrahydrofuran to obtain 1.4 g of polylithiated ferrocene lithium salt;
[0014] B2: The lithium ferrocenium salt obtained in step B1 was completely dissolved in 120 ml of tetrahydrofuran under nitrogen protection, 23 g of hexamethylcyclotrisiloxane and 0.2 ml of 12-4 crown ether were added to the solution, and the reaction was carried out at room temperature for 1 hour, and then the reaction solution was added dropwise to 50 ml of tetrahydrofuran containing 18 g of dimethyldichlorosilane for 1 hour, and stirred at room temperature for 12 hours;
[0015] B3 removing unreacted dimethyldichlorosilane and solvent under vacuum conditions, extracting the reaction product with toluene to obtain a polymer containing silicon-chloride end groups;
[0016] B4: Add the polymer containing silicon-chloride end groups obtained in step 3 into toluene at a concentration of 30%, then introduce ammonia gas at room temperature until there is no obvious ammonia absorption, then raise the temperature to 80°C and continue to introduce ammonia gas for 2 hours to obtain a ferrocenylsilazane crosslinking agent.
[0017] The present invention also provides a method for preparing high temperature resistant room temperature curing silicone rubber, comprising the following steps:
[0018] S1: 100 phr of hydroxyl-terminated polydimethylsiloxane (PDMS) and 20 phr of white carbon black are mixed evenly on a mixer;
[0019] S2: add 5-20 phr of ferrocenylsilazane crosslinking agent to the mixture of step S1 and mix well, then add 0.2 phr of dibutyltin dilaurate and stir at room temperature until the mixture is well mixed;
[0020] S3: pouring the mixture of step S2 into a mold, removing bubbles under vacuum, and then curing at room temperature to obtain high temperature resistant room temperature curing silicone rubber.
[0021] Preferably, the ferrocenylsilazane crosslinking agent is prepared by the above preparation method.
[0022] Preferably, the mixer is a three-roll mixer.
[0023] Preferably, the curing time in step S3 is 7-10 days.
[0024] The present invention also provides a high temperature resistant room temperature curing silicone rubber, which is prepared from the following raw materials in parts by weight: 100 phr hydroxyl-terminated polydimethylsiloxane (PDMS), 20 phr white carbon black, 0.2 phr dibutyltin dilaurate, and 1-20 phr ferrocenesilazane crosslinking agent (FSCA).
[0025] Preferably, the silicone rubber is prepared by the above preparation method.
[0026] Preferably, the ferrocenylsilazane crosslinking agent is prepared by the above preparation method.
[0027] The technical solution provided by the present invention brings beneficial effects:
[0028] The room temperature vulcanized silicone rubber crosslinking agent of the present invention mainly solves the stability problem of silicone rubber under high temperature conditions, especially by introducing the structure of ferrocene and silicon nitrogen bond, the performance of silicone rubber under extreme temperature is significantly improved. In the traditional silicone rubber system, the main chain breaks rapidly due to thermal degradation under high temperature, especially in the presence of uncrosslinked hydroxyl groups and adsorbed water, these factors together lead to the decline of material performance. The silicon nitrogen bond used in the present invention can effectively eliminate the silicon hydroxyl groups in the system, reduce the main chain breakage caused by thermal degradation, and thus improve the thermal stability of silicone rubber.
[0029] The introduction of silicon-nitrogen bonds improves the stability of silicone rubber at high temperatures. In existing silicone rubber systems, silanol groups are prone to breakage or participate in undesirable side reactions at high temperatures, while the presence of silicon-nitrogen bonds effectively prevents this process. This structural improvement allows silicone rubber to maintain its mechanical properties and chemical stability even in a continuous high-temperature environment, extending the service life of the material.
[0030] The introduction of ferrocene further enhances the antioxidant capacity of silicone rubber. In an environment with high temperature and oxygen, ordinary silicone rubber is prone to oxidation, resulting in rapid degradation of physical properties. Ferrocene, due to its unique chemical structure, can effectively capture free radicals and slow down the oxidation process, thereby improving the high temperature oxidation stability of silicone rubber without adding additional antioxidants.
[0031] The present invention realizes the possibility of using silicone rubber in air atmosphere by synthesizing a room temperature vulcanized silicone rubber crosslinking agent with ferrocene as the core and silicon nitrogen bond as the crosslinking group. Traditional silicone rubber needs additional antioxidants to ensure performance when used in air, while the crosslinking agent of the present invention achieves the same effect through its inherent chemical structure. This not only reduces the complexity of material preparation, but also improves the economic benefits and environmental adaptability of the material in practical applications.
[0032] In summary, the room temperature vulcanized silicone rubber crosslinking agent of the present invention significantly improves the performance and stability of silicone rubber in high temperature and oxidative environments, and these technical effects directly respond to the problem of silicone rubber performance degradation in high temperature environments in the prior art. Through these technical improvements, the present invention has important practical and theoretical significance in improving the application range and service life of silicone rubber. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The effect of FSCA content on isothermal thermal weight loss of vulcanized rubber in the present invention;
[0034] Figure 2 The effect of the FSCA content of the present invention on the tensile strength of the vulcanized rubber after aging;
[0035] Figure 3This is a photo of ferrocenylsilazane crosslinker. DETAILED DESCRIPTION
[0036] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Of course, the specific embodiments described here are only used to explain the present invention and are not used to limit the present invention.
[0037] Example 1
[0038] The present invention provides a ferrocenylsilazane (FSCA) crosslinking agent, and the specific scheme is as follows:
[0039] The cross-linking agent is prepared by the following steps:
[0040] B1 Under nitrogen protection, 1.86 g, 0.01 mol of ferrocene and 20 ml of n-hexane were mixed and stirred until completely dissolved, 62.5 ml of n-hexane solution containing 0.1 mol of butyl lithium and 11.2 ml of tetramethylethylenediamine were added to the above solution, the reaction mixture was heated to n-hexane reflux, and the reaction was stirred for 10 hours, then the upper solution was filtered and removed, the precipitate was washed with 40 ml of n-hexane, and the obtained precipitate was recrystallized using tetrahydrofuran to obtain 1.4 g of polylithiated ferrocene lithium salt;
[0041] B2: The lithium ferrocenium salt obtained in step B1 was completely dissolved in 120 ml of tetrahydrofuran under nitrogen protection, 23 g of hexamethylcyclotrisiloxane and 0.2 ml of 12-4 crown ether were added to the solution, and the reaction was carried out at room temperature for 1 hour, and then the reaction solution was added dropwise to 50 ml of tetrahydrofuran containing 18 g of dimethyldichlorosilane for 1 hour, and stirred at room temperature for 12 hours;
[0042] B3 removing unreacted dimethyldichlorosilane and solvent under vacuum conditions, extracting the reaction product with toluene to obtain a polymer containing silicon-chloride end groups;
[0043] B4: Add the polymer containing silicon-chloride end groups obtained in step 3 into toluene at a concentration of 30%, then introduce ammonia gas at room temperature until there is no obvious ammonia absorption, then raise the temperature to 80°C and continue to introduce ammonia gas for 2 hours to obtain a ferrocenylsilazane crosslinking agent.
[0044] A method for preparing high temperature resistant room temperature curing silicone rubber comprises the following steps:
[0045] S1: 100 phr of hydroxyl-terminated polydimethylsiloxane (PDMS) and 20 phr of fumed silica were mixed evenly on a three-roll mixer;
[0046] S2: add 10 phr of ferrocenylsilazane crosslinking agent to the mixture of step S1 and mix well, then add 0.2 phr of dibutyltin dilaurate and stir at room temperature until the mixture is well mixed;
[0047] S3: pouring the mixture of step S2 into a mold, removing bubbles under vacuum, and then curing at room temperature for 7 days to obtain high temperature resistant room temperature curing silicone rubber.
[0048] Example 2
[0049] The preparation was carried out in the same manner as in Example 1, except that the molar ratio of ferrocene to butyl lithium was 1:5.
[0050] Example 3
[0051] The preparation was carried out in the same manner as in Example 1, except that the molar ratio of ferrocene to butyl lithium was 1:15.
[0052] Example 4
[0053] The preparation was carried out in the same manner as in Example 1, except that in step S2, 5 phr of ferrocenylsilazane crosslinking agent was added.
[0054] Example 5
[0055] The preparation was carried out in the same manner as in Example 1, except that, in step S2, 15 phr of ferrocenylsilazane crosslinking agent was added.
[0056] Example 6
[0057] The preparation is carried out in the same manner as in Example 1, except that in step S3, the curing time is 10 days.
[0058] Comparative Example 1
[0059] The preparation was carried out in the same manner as in Example 1, except that the ferrocenylsilazane crosslinking agent was replaced by tetraethyl orthosilicate crosslinking agent.
[0060] Experimental test:
[0061] 1. Mechanical properties: According to the national standard GB528-98, the prepared vulcanized rubber samples were cut into dumbbell-shaped specimens and subjected to room temperature tensile tests on an Instron 5565 universal electronic material testing machine. The length between the clamps was 10 mm and the tensile rate was 200 mm / min.
[0062] 2. Isothermal thermal weight loss: Place the silicone rubber in a hot air circulation aging box for thermal oxygen aging at a temperature of 300°C for 24 hours. The ratio of the weight loss of the sample to the initial weight is the isothermal thermal weight loss.
[0063] 3. Hot air aging:
[0064] The aging temperature was 300°C and the atmosphere was air.
[0065] Table 1 Mechanical properties test data
[0066]
[0067] As can be seen from the table, after cross-linking with ferrocenesilazane crosslinker, the tensile strength and elongation at break of the prepared silicone rubber are higher than those of the silicone rubber prepared with tetraethyl orthosilicate as crosslinker. After high-temperature aging at 300℃×24 hours, the silicone rubber cross-linked with tetraethyl orthosilicate has lost its physical and mechanical properties and cannot be tested, while the silicone rubber cross-linked with ferrocenesilazane crosslinker still has good tensile strength after vulcanization. After high-temperature aging at 300℃×24 hours, the silicone rubber cross-linked with ferrocenesilazane crosslinker has a smaller weight loss than the silicone rubber cross-linked with tetraethyl orthosilicate.
[0068] When the amount of FSCA is less than 5phr, the vulcanized rubber cannot be fully vulcanized, and the amount of FSCA should be greater than 5phr.
[0069] Isothermal thermal weight loss performance is one of the important indicators of silicone rubber's thermal oxidation stability. At high temperatures, the residual silanol groups in silicone rubber will cause degradation and weight loss. In addition, the oxidation of silicone rubber and the silanol groups produced by oxidation will cause thermal weight loss of the system. The silicon-nitrogen bond can eliminate the silanol groups in the system, and the ferrocene group will inhibit the thermal oxidation of the methyl group in the system. Figure 1 The isothermal thermal oxidation weight loss of vulcanized rubber with FSCA dosage of 10 and 15 phr and that of vulcanized rubber with crosslinking agent ethyl orthosilicate dosage of 10 phr at different times was compared. Figure 1 The isothermal thermal weight loss curves of the vulcanized rubber under 300°C air atmosphere are compared. As can be seen from the figure, with the increase of aging time, the thermal weight loss of the vulcanized rubber gradually increases, but the slope of the thermal aging curve gradually decreases, indicating that the rate of thermal weight loss gradually decreases. The thermal weight loss of the vulcanized rubber cross-linked with FSCA is lower than that of the vulcanized rubber with tetraethyl orthosilicate as the cross-linking agent. The weight loss changes of the vulcanized rubber with FSCA dosages of 10 and 15phr are basically the same. After aging for 24 hours, the weight loss of the vulcanized rubber cross-linked with 10phr silazane is 12%, while the weight loss of the vulcanized rubber cross-linked with the same amount of TEOS is 15%.
[0070] Figure 2The effect of aging time on the tensile strength of vulcanized rubber. As can be seen from the figure, at the same time, the tensile strength of the vulcanized rubber with FSCA of 10phr is greater than that of the vulcanized rubber with FSCA of 15phr. The aging time is 24 hours, and the tensile strength of the former is 2.4MPa, while that of the latter is 1.4MPa. With the increase of aging time, the tensile strength of the vulcanized rubber first decreases and then remains basically unchanged. The decrease in tensile strength at the initial stage of aging is caused by the depolymerization of the molecular chain, which is consistent with the large initial thermal weight loss rate. With the increase of time, the tensile strength remains stable. However, the silicone rubber with only TEOS added was severely oxidized after 300℃*24h and the mechanical properties could not be tested.
[0071] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A ferrocenylsilazane crosslinking agent, characterized in that The cross-linking agent is prepared by the following steps: A1, under nitrogen protection, ferrocene and n-hexane are mixed and stirred until completely dissolved, n-hexane solution of butyl lithium and tetramethylethylenediamine are added to the above solution, the reaction mixture is heated to n-hexane reflux, and the reaction is continuously stirred, then the upper solution is filtered and removed, the precipitate is washed with n-hexane, and the obtained precipitate is recrystallized using tetrahydrofuran to obtain polylithiated ferrocene lithium salt; A2: adding tetrahydrofuran to completely dissolve the lithium ferrocenium salt obtained in step A1 under nitrogen protection, adding hexamethylcyclotrisiloxane and 12-4 crown ether to the solution, reacting at room temperature, then dropping the reaction solution into tetrahydrofuran containing dimethyldichlorosilane, and stirring at room temperature; A3 removes unreacted dimethyldichlorosilane and solvent under vacuum conditions, and extracts the reaction product with toluene to obtain a polymer containing silicon-chloride terminal groups; A4: passing ammonia gas into the toluene solution obtained in step A3 at room temperature until no obvious ammonia gas absorption occurs, and then increasing the temperature and continuing to pass ammonia gas, thereby obtaining a ferrocenylsilazane crosslinking agent.
2. The ferrocenylsilazane crosslinking agent according to claim 1, characterized in that The molar ratio of ferrocene to butyl lithium is 1:5-1:
15.
3. The ferrocenylsilazane crosslinking agent according to claim 2, characterized in that The preparation method of the cross-linking agent corresponding to each 1.86g of ferrocene is: B1 Under nitrogen protection, 1.86 g, 0.01 mol of ferrocene and 20 ml of n-hexane were mixed and stirred until completely dissolved, 62.5 ml of n-hexane solution containing 0.1 mol of butyl lithium and 11.2 ml of tetramethylethylenediamine were added to the above solution, the reaction mixture was heated to n-hexane reflux, and the reaction was stirred for 10 hours, then the upper solution was filtered and removed, the precipitate was washed with 40 ml of n-hexane, and the obtained precipitate was recrystallized using tetrahydrofuran to obtain 1.4 g of polylithiated ferrocene lithium salt; B2: The lithium ferrocenium salt obtained in step B1 was completely dissolved in 120 ml of tetrahydrofuran under nitrogen protection, 23 g of hexamethylcyclotrisiloxane and 0.2 ml of 12-4 crown ether were added to the solution, and the reaction was carried out at room temperature for 1 hour, and then the reaction solution was added dropwise to 50 ml of tetrahydrofuran containing 18 g of dimethyldichlorosilane for 1 hour, and stirred at room temperature for 12 hours; B3 removing unreacted dimethyldichlorosilane and solvent under vacuum conditions, extracting the reaction product with toluene to obtain a polymer containing silicon-chloride end groups; B4: Add the polymer containing silicon-chloride end groups obtained in step 3 into toluene at a concentration of 30%, then introduce ammonia gas at room temperature until there is no obvious ammonia absorption, then raise the temperature to 80°C and continue to introduce ammonia gas for 2 hours to obtain a ferrocenylsilazane crosslinking agent.
4. A method for preparing high temperature resistant room temperature curing silicone rubber, characterized in that: The following steps are involved: S1: 100 phr of hydroxyl-terminated polydimethylsiloxane and 20 phr of white carbon black are mixed evenly on a mixer; S2: add 5-20 phr of ferrocenylsilazane crosslinking agent to the mixture of step S1 and mix well, then add 0.2 phr of dibutyltin dilaurate and stir at room temperature until the mixture is well mixed; S3: pouring the mixture of step S2 into a mold, removing bubbles under vacuum, and then curing at room temperature to obtain high temperature resistant room temperature curing silicone rubber.
5. The preparation method according to claim 4, characterized in that: The ferrocenylsilazane crosslinking agent is prepared by the preparation method of claim 1.
6. The preparation method according to claim 4, characterized in that: The mixing mill is a three-roll mixing mill.
7. The preparation method according to claim 4, characterized in that: The curing time in step S3 is 7-10 days.
8. A high temperature resistant room temperature curing silicone rubber, characterized in that: The silicone rubber is prepared from the following raw materials in parts by weight: 100 phr of hydroxyl-terminated polydimethylsiloxane, 20 phr of white carbon black, 0.2 phr of dibutyltin dilaurate, and 1-20 phr of ferrocenylsilazane crosslinking agent.
9. The high temperature resistant room temperature curing silicone rubber according to claim 8, characterized in that: The silicone rubber is prepared by the preparation method described in claim 4.
10. The high temperature resistant room temperature curing silicone rubber according to claim 8, characterized in that: The ferrocenylsilazane crosslinking agent is prepared by the preparation method of claim 1.
Citation Information
Patent Citations
Ternary catalyst system containing PNN structure skeleton ligand, and applications thereof
CN106853378A
Polymer precursor ceramic composite aerogel and microwave synthesis method thereof
CN108341674A
Compound and production method therefor
WO2021024675A1
Cited By
Organic silicon modified heat-resistant flame retardant, preparation method thereof and application of organic silicon modified heat-resistant flame retardant in silicone rubber
CN120554707A
Organic silicon high-temperature-resistant cross-linking agent as well as preparation method and application thereof
CN122277605A