Polyphosphazene modified montmorillonite flame retardant and preparation method thereof
By preparing polyphosphazene-modified montmorillonite flame retardant, the problem of flammability of PET materials is solved. By diluting oxygen and suppressing melt droplets, the flame retardancy of PET composite materials is significantly improved, reaching V-0 level flame retardancy. grade, and improves the mechanical properties of the material.
Patent Information
- Application Number
- CN202410996785.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
AI Technical Summary
PET materials are flammable, and existing technologies cannot effectively improve their flame retardancy, and cyclotriphosphazene produces harmful gases when burned, affecting material performance.
The preparation method of polyphosphazene-modified montmorillonite flame retardant is used to generate cyclic cross-linked polyphosphazene microspheres through the nucleophilic substitution reaction of tetrachlorocyclotriphosphazene and 4,4'-diaminodiphenylmethane. , and then reacted with modified montmorillonite through the intercalation reaction of silane coupling agent and quaternary phosphorus salt to form PHM-OMMT flame retardant, which is used in PET composite materials.
Significantly improves the flame retardancy of PET composite materials, by diluting oxygen and suppressing droplets, extending the burning time, reaching a V-0 level flame retardant grade, and improving the mechanical properties of the material.
Smart Images

Figure CN118755151A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of flame retardants, and in particular to a polyphosphazene modified montmorillonite flame retardant and a preparation method thereof. Background Art
[0002] PET is a non-toxic, corrosion-resistant, and dimensionally stable compound. It is considered one of the most important polymer materials at this stage because of its many advantages. However, PET is a flammable material that produces a lot of smoke and serious droplets during combustion, which poses a huge safety hazard to people's lives and production.
[0003] As a new type of organic phosphorus flame retardant skeleton material, cyclotriphosphazene has a stable six-membered ring conjugated structure and a high phosphorus and nitrogen content. Its derivatives have the excellent properties of both inorganic and organic substances. However, cyclotriphosphazene produces hydrogen chloride gas when burned, which can cause secondary damage to the human body, and is easily hydrolyzed, resulting in a decrease in the mechanical properties of the material, so it needs to be modified.
[0004] Montmorillonite is cheap and has excellent performance. The flakes of organic modified montmorillonite can play a certain barrier role inside the polymer, slowing down and hindering the migration of small molecular combustible substances during the combustion process, and slowing down the penetration of external oxygen into the material, making it difficult for the oxidation reaction to proceed fully, thus playing a flame retardant role. However, there are a large number of inorganic ions between the layers of montmorillonite, and its compatibility with organic compounds is poor. Summary of the invention
[0005] The problem in the prior art is that PET does not have flame retardancy. In view of the above problem, the present invention provides a polyphosphazene modified montmorillonite flame retardant, and the preparation method thereof comprises the following steps:
[0006] (1) Synthesis of PHM microspheres:
[0007] The H atom on the amino group in the molecular structure of 4,4'-diaminodiphenylmethane and some Cl atoms connected to the phosphorus atom in the molecular structure of hexachlorocyclotriphosphazene undergo a nucleophilic substitution reaction under the action of an acid binding agent. After the reaction is completed, ring-crosslinked polyphosphazene microspheres, namely PHM microspheres, are obtained. The amount ratio of hexachlorocyclotriphosphazene to 4,4'-diaminodiphenylmethane in the reaction is 0.35g:0.2g-0.35g:1.0g.
[0008] (2) Synthesis of AP-MMT:
[0009] The silanol generated by the hydrolysis of 3-aminopropyltriethoxysilane (APTES) reacts with the hydroxyl groups on the surface of sodium montmorillonite (Na-MMT) to form Si-O-Si bonds. After the reaction, silane coupling agent-modified montmorillonite, namely AP-MMT, is obtained.
[0010] (3) Synthesis of OMMT:
[0011] AP-MMT and BPP undergo a cation exchange reaction, and the quaternary phosphorus ions are intercalated into the montmorillonite layers in the AP-MMT molecular structure. After the reaction is completed, a quaternary phosphorus salt intercalated modified montmorillonite, namely OMMT, is obtained.
[0012] (4) Synthesis of PHM-OMMT:
[0013] The H atom on the amino group of the silane coupling agent chain segment in the OMMT structure and the Cl atom connected to the phosphorus atom in the PHM microsphere structure undergo a nucleophilic substitution reaction under the action of the acid binding agent. After the reaction is completed, a polyphosphazene modified montmorillonite flame retardant, namely PHM-OMMT, is obtained.
[0014] Preferably, the solvent for the nucleophilic substitution reaction in step (1) comprises acetonitrile or tetrahydrofuran.
[0015] Preferably, the solvent used for the dehydration condensation reaction in step (2) is a mixed solution of ethanol and water, and the volume ratio of ethanol to water is 7:3-9:1.
[0016] Preferably, the solvent used in the cation exchange reaction in step (3) includes water and ethanol.
[0017] Preferably, the solvent for the nucleophilic substitution reaction in step (4) comprises acetonitrile or tetrahydrofuran.
[0018] Preferably, the acid binding agent includes triethylamine, pyridine, and potassium carbonate.
[0019] Preferably, the method of step (1) comprises the following steps:
[0020] (1) dissolving 4,4'-diaminodiphenylmethane in a solvent, then starting to drop an acid-binding agent, and uniformly dispersing the reaction system by ultrasonication; the amount ratio of 4,4'-diaminodiphenylmethane to the acid-binding agent and the solvent in the reaction is 0.2 g:40 mL:3 mL-1.0 g:50 mL:5 mL;
[0021] (2) dissolving hexachlorocyclotriphosphazene in a solvent, and then adding the solvent to the reaction system formed in step (1), stirring and reacting at 60° C.-80° C. for 18 h-24 h. After the reaction is completed, centrifuging, washing and drying the reaction solution to obtain PHM; the ratio of hexachlorocyclotriphosphazene to the solvent in the reaction is 0.35 g:40 mL-0.35:50 mL.
[0022] Preferably, the method of step (2) comprises the following steps:
[0023] Na-MMT and APTES are added to the solvent, stirred and hydrolyzed at 40°C-60°C for 100min-120min. After the reaction, the suspension is centrifuged and washed at least three times. The solid product is dried at 50°C-60°C for 18h-24h to obtain AP-MMT. The dosage ratio of Na-MMT to APTES and solvent in the reaction is 1g:0.8mL:100mL-1g:1.2mL:100mL.
[0024] Preferably, the method of step (3) comprises the following steps:
[0025] (1) Add AP-MMT to deionized water and stir at a constant temperature of 60°C-80°C for 3.5h-4.5h; during the reaction, the ratio of AP-MMT to deionized water is 1.0g:100mL-1.25g:100mL;
[0026] (2) dissolving triphenylbenzyl phosphonium chloride in deionized water in a ratio of 0.7 g:10 mL, and then adding the solution to the reaction system formed in step (1), stirring the solution at a constant temperature of 70° C. to 80° C. for 8 h to 10 h. After the reaction is completed, centrifuging the reaction solution, and then washing with deionized water and ethanol in sequence until the supernatant of the washing solution cannot change the color of the 0.1 mol / L AgNO3 solution. Then, stopping washing, collecting the solid product and drying it to obtain OMMT.
[0027] Preferably, the method of step (4) comprises the following steps:
[0028] PHM is evenly dispersed in a solvent, and then OMMT is added to the reaction system, stirred and dispersed evenly, and then an acid binding agent is added to the reaction system, and the reaction is stirred at 60°C-80°C for 18h-24h. The amount ratio of PHM to OMMT and the acid binding agent in the reaction is 0.3g:0.2g:3mL-0.5g:0.6g:5mL; after the reaction is completed, the reaction system is centrifuged, washed, and vacuum dried to obtain PHM-OMMT.
[0029] The present invention has the following beneficial effects:
[0030] (1) The present invention provides a flame retardant PHM-OMMT, wherein the molecular structure of the flame retardant PHM-OMMT contains a ring-crosslinked polyphosphazene microsphere structure PHM and a quaternary phosphonium salt intercalated modified montmorillonite structure OMMT, and the OMMT structure is linked to the PHM microsphere structure through an NP bond. The flame retardant PHM-OMMT obtained by the present invention is used as a flame retardant for a PET composite material, which can significantly improve the flame retardancy of the PET composite material;
[0031] (2) The flame retardant PHM-OMMT obtained by the present invention contains a large amount of amino groups in its structure. During the combustion process, ammonia gas is generated to dilute the oxygen around the PET composite material, and molten droplets are generated to inhibit the transfer of flames and heat, which is very beneficial to improving the flame retardancy of the PET composite material;
[0032] (3) The OMMT structure in the flame retardant PHM-OMMT obtained by the present invention is a montmorillonite structure modified by quaternary phosphonium salt intercalation. The montmorillonite modified by quaternary phosphonium salt intercalation has a larger interlayer spacing, which can better slow down and hinder the migration of small molecular combustible substances in the combustion process inside the polymer, and at the same time slow down the penetration of external oxygen into the material, making it difficult for the oxidation reaction to proceed fully, which is very beneficial to improving the flame retardancy of the obtained PET composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 : Infrared spectra of PHM, OMMT and PHM-OMMT obtained in Example 1 of the present invention.
[0034] Figure 2 : SEM image of the flame retardant PHM-OMMT obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0035] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0036] Example 1
[0037] A polyphosphazene modified montmorillonite flame retardant, the preparation method is as follows:
[0038] Synthesis of PHM microspheres:
[0039] (1) dissolving 4,4'-diaminodiphenylmethane in acetonitrile, and then beginning to dropwise add triethylamine, and ultrasonically dispersing the reaction system uniformly; the amount ratio of 4,4'-diaminodiphenylmethane to triethylamine and acetonitrile in the reaction is 0.8 g:50 mL:4 mL;
[0040] (2) dissolving hexachlorocyclotriphosphazene in acetonitrile in a ratio of 0.35 g to 50 mL of hexachlorocyclotriphosphazene and then adding the mixture to the reaction system formed in step (1) and stirring the mixture at 70° C. for 18 h. After the reaction, centrifuging the reaction solution to obtain a solid product. The solid product was washed three times with acetonitrile and three times with deionized water respectively, and then vacuum dried at 60° C. for 12 h to obtain PHM as a yellow powder.
[0041] Synthesis of AP-MMT:
[0042] Na-MMT and APTES were added into a mixed solvent consisting of ethanol and deionized water in a volume ratio of 9:1, and hydrolyzed at 50°C with stirring for 120 min. After the reaction, the suspension was centrifuged and washed at least three times. The solid product was dried at 60°C for 18 h to obtain AP-MMT. The dosage ratio of Na-MMT to APTES and solvent in the reaction was 1 g:1 mL:100 mL.
[0043] Synthesis of OMMT:
[0044] (1) AP-MMT was added to deionized water and stirred at 70°C for 4 h. During the reaction, the ratio of AP-MMT to deionized water was 1.25 g:100 mL.
[0045] (2) Dissolve triphenylbenzyl phosphonium chloride in deionized water in a ratio of 0.7 g:10 mL, then add the solution to the reaction system formed in step (1), and stir at 70° C. for 8 h. After the reaction, centrifuge the reaction solution, and then repeatedly wash with deionized water and ethanol until the supernatant of the washing solution cannot change the color of the 0.1 mol / L AgNO3 solution. Stop washing, collect the solid product and dry it to obtain OMMT.
[0046] Synthesis of PHM-OMMT:
[0047] PHM was evenly dispersed in tetrahydrofuran, and then OMMT was added to the reaction system, and stirred to disperse evenly. Then, an acid binding agent was added to the reaction system, and the reaction was stirred at 70°C for 18 hours.
[0048] The dosage ratio of PHM to OMMT and acid binding agent in the reaction is 0.3 g:0.2 g:3 mL;
[0049] After the reaction was completed, the reaction system was centrifuged, washed twice with tetrahydrofuran, washed once with deionized water, and dried under vacuum at 60° C. for 24 h to obtain PHM-OMMT.
[0050] Instructions attached Figure 1 The infrared spectra of PHM, OMMT and PHM-OMMT obtained in Example 1 are shown in FIG. In the spectra, two phenyl characteristic absorption peaks are retained in the structure of PHM, 1175 cm -1 The absorption peak is the stretching vibration of the P=N bond (the structure on HCCP is retained here), 1018cm -1 The characteristic peak at 1451cm indicates that a new -P-NH- bond is formed in PHM. This shows that the polyphosphazene microspheres were successfully prepared. -1 A new peak appeared at 694cm-1 A new peak appeared at 1040 cm -1 The Si-O stretching vibration peak still exists, which indicates that the modifier is successfully intercalated into the montmorillonite layer. Comparing the infrared spectra of PHM and OMMT, it can be seen that PHM-OMMT retains the PHM at 1512cm -1 The characteristic absorption peak of phenyl at 1167cm -1 The stretching vibration peak of the P=N bond at 694cm in the OMMT structure is also retained. -1 The CH bending vibration peak in the benzene ring appears at 1039cm -1 The stretching vibration peak of Si-O at 1.37° is shown in Figure 2. It can be seen that PHM-OMMT was successfully prepared, and it has the structure of both ring-crosslinked polyphosphazene and montmorillonite.
[0051] Instructions attached Figure 2 This is a SEM image of PHM-OMMT obtained in Example 1. In the image, a smooth surface of polyphosphazene microsphere structure and a montmorillonite lamellar structure can be seen.
[0052] Specific applications
[0053] Preparation of PET / PHM-OMMT composites:
[0054] The PET pellets were dried at 120°C for 12 h, and then PHM-OMMT was added to PET and blended evenly using an internal mixer. The temperature of the internal mixer was set at 260-270°C and the speed was set at 40-60 r / min to obtain a PET / PHM-OMMT composite material with a PHM-OMMT content of 0.5 wt%.
[0055] Example 2 is the same as Example 1, except that in Example 2, the amount of PHM-OMMT added to PET is 1.0 wt%.
[0056] Example 3 is the same as Example 1, except that in Example 3, the amount of PHM-OMMT added to PET is 1.5 wt%.
[0057] Example 4 is the same as Example 1, except that in Example 4, the amount of PHM-OMMT added to PET is 2.0 wt%.
[0058] Comparative Example 1 is the same as Example 1, except that PHM-OMMT is not added in Comparative Example 1, and pure PET material is obtained after mixing.
[0059] Comparative Example 2 is the same as Example 2, except that in Comparative Example 2, the PHM-OMMT added during the preparation of the PET / PHM-OMMT composite material is replaced with hexachlorocyclotriphosphazene of equal mass.
[0060] Comparative Example 3 is the same as Example 1, except that in Comparative Example 3, the PHM-OMMT added during the preparation of the PET / PHM-OMMT composite material is replaced with PHM of equal mass.
[0061] Comparative Example 4 is the same as Example 2, except that in Comparative Example 4, the PHM-OMMT added in the preparation process of the PET / PHM-OMMT composite material is replaced by PHM, and the addition amount of PHM in PET is 1.0 wt%.
[0062] Comparative Example 5 is the same as Example 3, except that in Comparative Example 5, the PHM-OMMT added in the preparation process of the PET / PHM-OMMT composite material is replaced by PHM, and the addition amount of PHM in PET is 1.5 wt%.
[0063] Comparative Example 6 is the same as Example 4, except that in Comparative Example 6, the PHM-OMMT added in the preparation process of the PET / PHM-OMMT composite material is replaced by PHM, and the addition amount of PHM in PET is 2.0 wt%.
[0064] Comparative Example 7 is the same as Example 2, except that in Comparative Example 7, the PHM-OMMT added during the preparation of the PET / PHM-OMMT composite material is replaced with OMMT of equal mass.
[0065] Comparative Example 8 is the same as Example 4, except that in Comparative Example 8, the PHM-OMMT added during the preparation of the PET / PHM-OMMT composite material is replaced with OMMT of equal mass.
[0066] Comparative Example 9 is the same as Example 3, except that, in Comparative Example 9, the PHM-OMMT added during the preparation of the PET / PHM-OMMT composite material is replaced with a mixture of PHM and OMMT of equal mass in a mass ratio of 0.3 g:0.2 g.
[0067] Comparative Example 10 is the same as Example 3, except that, in Comparative Example 10, the PHM-OMMT added in the preparation process of the PET / PHM-OMMT composite material is replaced with polyphosphazene-modified montmorillonite of equal mass, and the polyphosphazene-modified montmorillonite is not modified by cationic quaternary phosphonium salt intercalation. The preparation method thereof is as follows:
[0068] PHM was evenly dispersed in tetrahydrofuran, and then AP-MMT was added to the reaction system, stirred and dispersed evenly, and then triethylamine was added to the reaction system, and the reaction was stirred at 70° C. for 18 hours.
[0069] The ratio of PHM to AP-MMT and triethylamine in the reaction was 0.3 g:0.2 g:3 mL;
[0070] After the reaction was completed, the reaction system was centrifuged, washed twice with tetrahydrofuran, washed once with deionized water, and vacuum dried at 60° C. for 24 h to obtain polyphosphazene modified montmorillonite.
[0071] Comparative Example 11 is the same as Example 3, except that the intercalation modifier used in the synthesis of OMMT in Comparative Example 11 is not BPP, but a cationic quaternary phosphonium salt modifier, dodecyl tributyl quaternary phosphonium salt.
[0072] Performance Testing
[0073] The PET composite materials obtained in Examples 1-4 of the present invention and Comparative Examples 1-11 were subjected to relevant performance tests, and the specific test results are shown in Table 1.
[0074] Limiting oxygen index: According to ASTM D 2863-97 standard, the test is carried out using the TM606 digital oxygen index tester; Vertical burning: According to UL 94-2013 standard, the test is carried out using a vertical burning tester.
[0075] Table 1
[0076]
[0077] As shown in Table 1, the limiting oxygen index value of pure PET is 22.5%, and t1 and t2 are both greater than 10s, and t1+t2 is greater than 30s, which shows that the flame retardant grade of pure PET is the lowest. When the PHM content is 0.5wt%, the limiting oxygen index of the composite material is 25.4%; when the PHM content is 2.0wt%, the limiting oxygen index of the composite material is 27.2%, which is higher than the limiting oxygen index of pure PET of 22.5%. When the addition amount of PHM-OMMT increases from 1.0wt% to 2.0wt%, the limiting oxygen index increases from 25.4% to 26.7%, proving the flame retardant effect of PHM-OMMT. When the addition amount of flame retardant PHM-OMMT is 2wt%, the limiting oxygen index of the composite material is 28.3%, the flame burning time t1 of the sample is only 0.79s, t2 is only 1.13s, the total flame burning time t1+t2 of each group of samples is only 1.92s, and the flame and flameless burning time t2+t3 of each sample after the second flame is only 1.33s. It can be seen that the flame retardancy of the PET composite material obtained by adding PHM-OMMT is better than that of the PET composite material obtained by adding PHM or OMMT to PET.
[0078] The t1 and t2 of the composite materials obtained in Examples 1-4 of the present invention are both less than 10s, the values of t1+t2 are also less than 50s, and t2+t3 are also less than 30s. These conditions meet the requirements of V-0 flame retardancy. However, since the drippings generated by the combustion of the composite materials in Examples 1 and 2 will ignite the absorbent cotton, the flame retardancy level can only reach V-2 level. The composite materials obtained in Examples 3 and 4 are not completely burned and the drippings generated do not ignite the absorbent cotton, indicating that their flame retardancy level has reached V-0 level.
[0079] As the amount of PHM added increases, the number of droplets generated during the combustion of the composite material increases. This may be due to the weak hydrogen bonds and π-π interactions between PHM and PET, which leads to the intensification of the droplet phenomenon. In addition, as the amount of flame retardant added increases, the amount of residual carbon will also increase after the composite material is burned. The large amount of droplets generated by the composite material during the combustion process can inhibit the transfer of flames and heat. At the same time, during the combustion process, PHM can decompose the non-flammable gas ammonia to dilute the oxygen around the material.
[0080] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A polyphosphazene modified montmorillonite flame retardant, characterized in that: The preparation method comprises the following steps: (1) Synthesis of PHM microspheres: The H atom on the amino group in the molecular structure of 4,4'-diaminodiphenylmethane and some Cl atoms connected to the phosphorus atom in the molecular structure of hexachlorocyclotriphosphazene undergo a nucleophilic substitution reaction under the action of an acid binding agent. After the reaction is completed, ring-crosslinked polyphosphazene microspheres, namely PHM microspheres, are obtained. The amount ratio of hexachlorocyclotriphosphazene to 4,4'-diaminodiphenylmethane in the reaction is 0.35g:0.2g-0.35g:1.0g. (2) Synthesis of AP-MMT: The silanol generated by the hydrolysis of APTES reacts with the hydroxyl groups on the surface of Na-MMT to form Si-O-Si bonds. After the reaction, silane coupling agent-modified montmorillonite, namely AP-MMT, is obtained. (3) Synthesis of OMMT: AP-MMT and BPP undergo a cation exchange reaction, and the quaternary phosphorus ions are intercalated into the montmorillonite layers in the AP-MMT molecular structure. After the reaction is completed, a quaternary phosphorus salt intercalated modified montmorillonite, namely OMMT, is obtained. (4) Synthesis of PHM-OMMT: The H atom on the amino group of the silane coupling agent chain segment in the OMMT structure and the Cl atom connected to the phosphorus atom in the PHM microsphere structure undergo a nucleophilic substitution reaction under the action of the acid binding agent. After the reaction is completed, a polyphosphazene modified montmorillonite flame retardant, namely PHM-OMMT, is obtained.
2. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The solvent for the nucleophilic substitution reaction in step (1) includes acetonitrile and tetrahydrofuran.
3. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The solvent used for the dehydration condensation reaction in step (2) is a mixed solution of ethanol and water, and the volume ratio of ethanol to water is 7:3-9:
1.
4. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The solvent used in the cation exchange reaction in step (3) includes water and ethanol.
5. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The solvent for the nucleophilic substitution reaction in step (4) includes acetonitrile and tetrahydrofuran.
6. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The acid binding agent includes triethylamine, pyridine and potassium carbonate.
7. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The method of step (1) comprises the following steps: (1) dissolving 4,4'-diaminodiphenylmethane in a solvent, then starting to drop an acid-binding agent, and uniformly dispersing the reaction system by ultrasonication; the amount ratio of 4,4'-diaminodiphenylmethane to the acid-binding agent and the solvent in the reaction is 0.2 g:40 mL:3 mL-1.0 g:50 mL:5 mL; (2) dissolving hexachlorocyclotriphosphazene in a solvent, and then adding the solvent to the reaction system formed in step (1), stirring and reacting at 60° C.-80° C. for 18 h-24 h. After the reaction is completed, centrifuging, washing and drying the reaction solution to obtain PHM; the ratio of hexachlorocyclotriphosphazene to the solvent in the reaction is 0.35 g:40 mL-0.35:50 mL.
8. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The method of step (2) comprises the following steps: Na-MMT and APTES are added to the solvent, stirred and hydrolyzed at 40°C-60°C for 100min-120min. After the reaction, the suspension is centrifuged and washed at least three times. The solid product is dried at 50°C-60°C for 18h-24h to obtain AP-MMT. The dosage ratio of Na-MMT to APTES and solvent in the reaction is 1g:0.8mL:100mL-1g:1.2mL:100mL.
9. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The method of step (3) comprises the following steps: (1) Add AP-MMT to deionized water and stir at a constant temperature of 60°C-80°C for 3.5h-4.5h; during the reaction, the ratio of AP-MMT to deionized water is 1.0g:100mL-1.25g:100mL; (2) dissolving triphenylbenzyl phosphonium chloride in deionized water in a ratio of 0.7 g:10 mL, and then adding the solution to the reaction system formed in step (1), stirring the solution at a constant temperature of 70° C. to 80° C. for 8 h to 10 h. After the reaction is completed, centrifuging the reaction solution, and then washing with deionized water and ethanol in sequence until the supernatant of the washing solution cannot change the color of the 0.1 mol / L AgNO3 solution. Then, stopping washing, collecting the solid product and drying it to obtain OMMT.
10. The polyphosphazene modified montmorillonite flame retardant according to claim 1, characterized in that: The method of step (4) comprises the following steps: PHM is evenly dispersed in a solvent, and then OMMT is added to the reaction system, stirred and dispersed evenly, and then an acid binding agent is added to the reaction system, and the reaction is stirred at 60°C-80°C for 18h-24h. The amount ratio of PHM to OMMT and the acid binding agent in the reaction is 0.3g:0.2g:3mL-0.5g:0.6g:5mL; after the reaction is completed, the reaction system is centrifuged, washed, and vacuum dried to obtain PHM-OMMT.
Citation Information
Cited By
Polyphosphazene modified polycarbodiimide flame-retardant anti-hydrolysis agent as well as preparation method and application thereof
CN119798685A