Scratch-resistant wear-resistant PP (polypropylene) functional plastic and preparation method thereof

By combining composite nano-anti-wear agent with polypropylene resin, anti-scratch and wear-resistant PP functional plastics are prepared, which solves the problem of insufficient wear resistance of polypropylene functional plastics and significantly improves its wear resistance and service life.

CN118755201APending Publication Date: 2024-10-11ZHEJIANG FULLSTAR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411142611.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing polypropylene functional plastics have poor wear resistance, resulting in reduced service life, especially in applications such as graters.

Method used

The composite nano-anti-wear agent is combined with polypropylene resin, and the composite nano-anti-wear agent is prepared by preparing emulsion, stirring, centrifugation, calcination and other steps, and then combined with polypropylene resin, plasticizer, stearate, antioxidant , dispersant is mixed, dried, melted, extruded and granulated to form scratch-resistant and wear-resistant PP functional plastic.

Benefits of technology

Significantly improves the wear resistance of polypropylene functional plastics, enhances its density and surface hardness, reduces wear, extends service life, and improves oxidation resistance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses an anti-scratch wear-resistant PP (polypropylene) functional plastic and a preparation method thereof. The anti-scratch wear-resistant PP functional plastic is prepared from the following components: polypropylene resin, a plasticizer, stearate, an antioxidant, a dispersing agent and a composite nano anti-wear agent. The polypropylene resin is isotactic polypropylene resin; the crystallinity of the isotactic polypropylene resin is 68-70%; the isotacticity of the isotactic polypropylene resin is 92-95%; the water absorption rate of the isotactic polypropylene resin is 0.01%-0.02%; according to the PP functional plastic prepared by the invention, the problem that the application of the PP functional plastic in some fields is limited due to the limitation of wear resistance can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of plastics, in particular to a scratch-resistant and wear-resistant PP functional plastic and a preparation method thereof. Background Art

[0002] With the continuous development of industry, polypropylene, as a high-performance functional plastic material, is playing an indispensable role in various industries with its unique advantages. From machinery, automobiles to electronic appliances, to construction and packaging industries, polypropylene has demonstrated its excellent performance and broad application prospects.

[0003] Polypropylene is a colorless, translucent, thermoplastic, lightweight general-purpose plastic with the characteristics of chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties, and good high-wear-resistant processing performance. Therefore, it is widely used in the packaging industry, automotive industry, electronics industry, construction industry, textile industry, etc. Among them, the grater is a common tool in the kitchen, and the choice of its material is crucial to the performance and user experience of the product. Among many materials, polypropylene (PP) has become one of the ideal choices for making graters due to its unique properties and wide applicability.

[0004] However, the wear resistance of polypropylene functional plastics prepared in the prior art is relatively poor, which causes it to be easily worn during use, resulting in a significant reduction in service life. Therefore, the present invention solves the corresponding problem by providing a scratch-resistant and wear-resistant PP functional plastic. Summary of the invention

[0005] The purpose of the present invention is to provide a scratch-resistant and wear-resistant PP functional plastic to solve the deficiencies in the prior art.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A scratch-resistant and wear-resistant PP functional plastic, comprising the following components by weight: 85-88 parts of polypropylene resin, 3-5 parts of plasticizer, 1-1.5 parts of stearate, 1-2 parts of antioxidant, 5-8 parts of dispersant, and 8-12 parts of composite nano anti-wear agent;

[0008] The polypropylene resin is an isotactic polypropylene resin;

[0009] The isotactic polypropylene resin has a crystallinity of 68-70%;

[0010] The isotactic polypropylene resin has an isotacticity of 92-95%;

[0011] The water absorption rate of the isotactic polypropylene resin is 0.01%-0.02%.

[0012] As a further technical solution: the preparation method of the composite nano anti-wear agent comprises the following steps:

[0013] (1) Preparation of emulsion:

[0014] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0015] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0016] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0017] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and aqueous ammonia were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion;

[0018] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution;

[0019] (3) centrifuging the reaction solution, filtering, washing, and drying to obtain a reaction material;

[0020] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent.

[0021] As a further technical solution: the mass fraction of the polyvinyl pyrrolidone hexanol solution in step (1) is 45%;

[0022] The mass fraction of the graphene dispersion is 3.5%;

[0023] The mass fraction of the sodium citrate solution is 10%;

[0024] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0025] As a further technical solution: in step (2), the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0026] As a further technical solution: the rotation speed of the centrifugal treatment in step (3) is 6000 r / min, and the centrifugal treatment time is 12 min;

[0027] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0028] The drying was performed at 65° C. for 10 hours.

[0029] As a further technical solution: in step (4), the calcination temperature is 550-580° C. and the calcination time is 2 hours.

[0030] As a further technical solution: in step (4), the inert atmosphere is either nitrogen or neon.

[0031] As a further technical solution: the plasticizer is diisononyl phthalate; the stearate is magnesium stearate;

[0032] The antioxidant is antioxidant 1010;

[0033] The dispersant is glyceryl tristearate.

[0034] As a further technical solution: the scratch-resistant and wear-resistant PP functional plastic is applied to a grater.

[0035] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0036] S1 Preparation:

[0037] Weigh the following according to weight: polypropylene resin, plasticizer, stearate, antioxidant, dispersant, composite nano anti-wear agent;

[0038] S2 Mixing:

[0039] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0040] Among them, the stirring and mixing speed is 500r / min;

[0041] The stirring time is 30 minutes;

[0042] S3 Dry:

[0043] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0044] Among them, the drying temperature is 80°C and the time is 1 hour;

[0045] S4 Granulation:

[0046] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0047] Beneficial effects:

[0048] The PP functional plastic prepared by the present invention effectively overcomes the limitation of traditional PP materials in terms of wear resistance by significantly improving its wear resistance, thereby expanding its application potential in multiple fields.

[0049] The present invention introduces a composite nano anti-wear agent into a polypropylene functional plastic. The introduced composite nano anti-wear agent can interact with the polypropylene molecular chain in a physical or chemical manner to form a composite material, which can effectively improve the wear resistance of the plastic.

[0050] The introduction of composite nano anti-wear agents can fill the gaps between polypropylene polymer molecules, thereby greatly increasing the density and surface hardness of polypropylene functional plastics, thereby improving its load-bearing capacity and surface scratch resistance. At the same time, the presence of composite nano anti-wear agents can also hinder the expansion of cracks, reduce the occurrence of wear, and improve the wear resistance of polypropylene functional plastics.

[0051] The partial graphene introduced into the composite nano anti-wear agent has a low friction coefficient and good lubrication properties, which can play a lubricating role in the friction process, reduce friction and wear rate, and in addition, can form a stable transfer film on the friction interface to further reduce friction and wear.

[0052] The strong interfacial bonding force that the composite nano anti-wear agent can form with the polypropylene molecular chain can improve the overall strength of the composite material. During the friction process, this strong interfacial bonding force can prevent the separation between the composite nano anti-wear agent and the matrix, maintain the integrity of the polypropylene functional plastic, and thus improve its wear resistance.

[0053] The introduction of antioxidants can greatly improve the antioxidant properties of polypropylene functional plastics, slow down the aging process of polypropylene functional plastics, and increase the service life of polypropylene functional plastics.

[0054] The grater processed by the material prepared by the present invention can greatly increase the service life of the grater. DETAILED DESCRIPTION

[0055] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0056] The following are specific embodiments

[0057] Example 1

[0058] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0059] S1 Preparation:

[0060] Weigh the following according to weight: 85 parts of polypropylene resin, 3 parts of diisononyl phthalate, 1 part of magnesium stearate, 10101 parts of antioxidant, 5 parts of tristearate glyceryl, and 8 parts of composite nano anti-wear agent;

[0061] The polypropylene resin is an isotactic polypropylene resin;

[0062] The crystallinity of isotactic polypropylene resin is 70%;

[0063] The isotacticity of isotactic polypropylene resin is 92%;

[0064] The water absorption rate of isotactic polypropylene resin is 0.01%.

[0065] The preparation method of the composite nano anti-wear agent comprises the following steps:

[0066] (1) First, prepare the emulsion:

[0067] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0068] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0069] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0070] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and ammonia water were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; the mass fraction of the polyvinyl pyrrolidone hexanol solution was 45%;

[0071] The mass fraction of the graphene dispersion is 3.5%;

[0072] The mass fraction of the sodium citrate solution is 10%;

[0073] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0074] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0075] (3) The reaction liquid is centrifuged, filtered, washed, and dried to obtain a reaction material; the centrifugal speed is 6000 r / min, and the centrifugal time is 12 min;

[0076] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0077] The drying was performed at 65° C. for 10 hours.

[0078] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent; the inert atmosphere is nitrogen.

[0079] S2 Mixing:

[0080] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0081] Wherein, the stirring and mixing speed is 500r / min;

[0082] The stirring time is 30 minutes;

[0083] S3 Dry:

[0084] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0085] The drying temperature is 80°C and the drying time is 1 hour;

[0086] S4 Granulation:

[0087] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0088] Example 2

[0089] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0090] S1 Preparation:

[0091] Weigh the following according to weight: 86 parts of polypropylene resin, 3.5 parts of diisononyl phthalate, 1.2 parts of magnesium stearate, 10101.5 parts of antioxidant, 6 parts of tristearate, and 10 parts of composite nano anti-wear agent;

[0092] The polypropylene resin is an isotactic polypropylene resin;

[0093] The crystallinity of isotactic polypropylene resin is 70%;

[0094] The isotacticity of isotactic polypropylene resin is 92%;

[0095] The water absorption rate of isotactic polypropylene resin is 0.01%.

[0096] The preparation method of the composite nano anti-wear agent comprises the following steps:

[0097] (1) First, prepare the emulsion:

[0098] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0099] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0100] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0101] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and ammonia water were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; the mass fraction of the polyvinyl pyrrolidone hexanol solution was 45%;

[0102] The mass fraction of the graphene dispersion is 3.5%;

[0103] The mass fraction of the sodium citrate solution is 10%;

[0104] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0105] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0106] (3) The reaction liquid is centrifuged, filtered, washed, and dried to obtain a reaction material; the centrifugal speed is 6000 r / min, and the centrifugal time is 12 min;

[0107] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0108] The drying was performed at 65° C. for 10 hours.

[0109] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent; the inert atmosphere is nitrogen.

[0110] S2 Mixing:

[0111] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0112] Among them, the stirring and mixing speed is 500r / min;

[0113] The stirring time is 30 minutes;

[0114] S3 Dry:

[0115] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0116] Among them, the drying temperature is 80°C and the time is 1 hour;

[0117] S4 Granulation:

[0118] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0119] Example 3

[0120] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0121] S1 Preparation:

[0122] Weigh the following according to weight: 86 parts of polypropylene resin, 3 parts of diisononyl phthalate, 1.5 parts of magnesium stearate, 10101 parts of antioxidant, 6 parts of tristearate, and 10 parts of composite nano anti-wear agent;

[0123] The polypropylene resin is an isotactic polypropylene resin;

[0124] The crystallinity of isotactic polypropylene resin is 70%;

[0125] The isotacticity of isotactic polypropylene resin is 92%;

[0126] The water absorption rate of isotactic polypropylene resin is 0.01%.

[0127] The preparation method of the composite nano anti-wear agent comprises the following steps:

[0128] (1) First, prepare the emulsion:

[0129] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0130] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0131] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0132] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and ammonia water were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; the mass fraction of the polyvinyl pyrrolidone hexanol solution was 45%;

[0133] The mass fraction of the graphene dispersion is 3.5%;

[0134] The mass fraction of the sodium citrate solution is 10%;

[0135] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0136] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0137] (3) The reaction liquid is centrifuged, filtered, washed, and dried to obtain a reaction material; the centrifugal speed is 6000 r / min, and the centrifugal time is 12 min;

[0138] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0139] The drying was performed at 65° C. for 10 hours.

[0140] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent; the inert atmosphere is nitrogen.

[0141] S2 Mixing:

[0142] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0143] Among them, the stirring and mixing speed is 500r / min;

[0144] The stirring time is 30 minutes;

[0145] S3 Dry:

[0146] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0147] Among them, the drying temperature is 80°C and the time is 1 hour;

[0148] S4 Granulation:

[0149] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0150] Example 4

[0151] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0152] S1 Preparation:

[0153] Weigh the following according to weight: 88 parts of polypropylene resin, 3 parts of diisononyl phthalate, 1.5 parts of magnesium stearate, 10101.5 parts of antioxidant, 6 parts of tristearate, and 11 parts of composite nano anti-wear agent;

[0154] The polypropylene resin is an isotactic polypropylene resin;

[0155] The crystallinity of isotactic polypropylene resin is 70%;

[0156] The isotacticity of isotactic polypropylene resin is 92%;

[0157] The water absorption rate of isotactic polypropylene resin is 0.01%.

[0158] The preparation method of the composite nano anti-wear agent comprises the following steps:

[0159] (1) First, prepare the emulsion:

[0160] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0161] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0162] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0163] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and ammonia water were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; the mass fraction of the polyvinyl pyrrolidone hexanol solution was 45%;

[0164] The mass fraction of the graphene dispersion is 3.5%;

[0165] The mass fraction of the sodium citrate solution is 10%;

[0166] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0167] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0168] (3) The reaction liquid is centrifuged, filtered, washed, and dried to obtain a reaction material; the centrifugal speed is 6000 r / min, and the centrifugal time is 12 min;

[0169] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0170] The drying was performed at 65° C. for 10 hours.

[0171] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent; the inert atmosphere is either nitrogen or neon.

[0172] S2 Mixing:

[0173] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0174] Wherein, the stirring and mixing speed is 500r / min;

[0175] The stirring time is 30 minutes;

[0176] S3 Dry:

[0177] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0178] The drying temperature is 80°C and the drying time is 1 hour;

[0179] S4 Granulation:

[0180] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0181] Example 5

[0182] A method for preparing scratch-resistant and wear-resistant PP functional plastic comprises the following steps:

[0183] S1 Preparation:

[0184] Weigh the following according to weight: 88 parts of polypropylene resin, 5 parts of diisononyl phthalate, 1.5 parts of magnesium stearate, 10102 parts of antioxidant, 8 parts of tristearate glyceryl, and 12 parts of composite nano anti-wear agent;

[0185] The polypropylene resin is an isotactic polypropylene resin;

[0186] The crystallinity of isotactic polypropylene resin is 70%;

[0187] The isotacticity of isotactic polypropylene resin is 92%;

[0188] The water absorption rate of isotactic polypropylene resin is 0.01%.

[0189] The preparation method of the composite nano anti-wear agent comprises the following steps:

[0190] (1) First, prepare the emulsion:

[0191] Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution;

[0192] Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion;

[0193] Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution;

[0194] To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and ammonia water were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; the mass fraction of the polyvinyl pyrrolidone hexanol solution was 45%;

[0195] The mass fraction of the graphene dispersion is 3.5%;

[0196] The mass fraction of the sodium citrate solution is 10%;

[0197] The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:3.

[0198] (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; the volume ratio of the emulsion to tetraethoxysilane is 5:1.

[0199] (3) The reaction liquid is centrifuged, filtered, washed, and dried to obtain a reaction material; the centrifugal speed is 6000 r / min, and the centrifugal time is 12 min;

[0200] Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes;

[0201] The drying was performed at 65° C. for 10 hours.

[0202] (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent; the inert atmosphere is either nitrogen or neon.

[0203] S2 Mixing:

[0204] Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture;

[0205] Among them, the stirring and mixing speed is 500r / min;

[0206] The stirring time is 30 minutes;

[0207] S3 Dry:

[0208] The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained;

[0209] Among them, the drying temperature is 80°C and the time is 1 hour;

[0210] S4 Granulation:

[0211] The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.

[0212] Comparative Example 1:

[0213] Based on the technical solution of Example 1, the difference from the technical solution of Example 1 is that no composite nano anti-wear agent is added.

[0214] Comparative Example 2:

[0215] Based on the technical solution of Example 1, the difference from the technical solution of Example 1 is that the composite nano anti-wear agent is replaced by an equal amount of silicon dioxide.

[0216] test:

[0217] The examples and comparative examples were injection molded by an injection molding machine to obtain samples with a size of 20 cm×15 cm×1 cm, and tested:

[0218] The surface hardness of the samples of the embodiment and the comparative example was measured using a XHRD-150 Rockwell hardness tester. Five points on the surface of each sample were selected for testing, and the average value was taken:

[0219] Table 1

[0220] Rockwell Hardness HRM Example 1 66 Example 2 65 Example 3 65 Example 4 66 Example 5 66 Comparative Example 1 60 Comparative Example 2 63

[0221] It can be seen from Table 1 that the PP functional plastic prepared by the present invention has a higher surface hardness. The improvement of the surface hardness can further improve the surface scratch resistance of the PP functional plastic.

[0222] The friction and wear test of the embodiment and the comparative example samples was carried out at room temperature and pressure using a HDM-20 friction and wear tester. The test time of each sample was 1.5 h, the rotation speed was 220 r / min, the load was 210 N, the dual ring material was 45# stainless steel, the outer diameter was 10 mm, and the inner diameter was 5 mm:

[0223] Table 2

[0224] Wear amount mg Example 1 4.22 Example 2 4.25 Example 3 4.31 Example 4 4.37 Example 5 4.56 Comparative Example 1 25.63 Comparative Example 2 14.71

[0225] It can be seen from Table 2 that the PP functional plastic prepared by the present invention has higher wear resistance.

[0226] The tensile strength of the samples of the examples and comparative examples was measured according to the test method in GB / T1040.2-2006 "Determination of tensile properties of plastics Part 2: Test conditions for molded and extruded plastics":

[0227] Table 3

[0228] Tensile strength MPa Example 1 35.06 Example 2 35.42 Example 3 35.15 Example 4 34.81 Example 5 35.68 Comparative Example 1 31.52 Comparative Example 2 32.34

[0229] It can be seen from Table 3 that the tensile properties of the PP functional plastic prepared by the present invention are improved.

[0230] The above description is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown. Any changes made in accordance with the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the specification, should be within the protection scope of the present invention.

Claims

1. A scratch-resistant and wear-resistant PP functional plastic, characterized in that: The composition includes the following components by weight: 85-88 parts of polypropylene resin, 3-5 parts of plasticizer, 1-1.5 parts of stearate, 1-2 parts of antioxidant, 5-8 parts of dispersant, and 8-12 parts of composite nano anti-wear agent; The polypropylene resin is an isotactic polypropylene resin; The isotactic polypropylene resin has a crystallinity of 68-70%; The isotactic polypropylene resin has an isotacticity of 92-95%; The water absorption rate of the isotactic polypropylene resin is 0.01%-0.02%.

2. The scratch-resistant and wear-resistant PP functional plastic according to claim 1, characterized in that: The preparation method of the composite nano antiwear agent comprises the following steps: (1) Preparation of emulsion: Adding polyvinyl pyrrolidone to hexanol, stirring and mixing evenly to obtain a polyvinyl pyrrolidone hexanol solution; Evenly dispersing graphene in anhydrous ethanol to obtain a graphene dispersion; Adding sodium citrate to deionized water, stirring and mixing evenly to obtain a sodium citrate solution; To the polyvinyl pyrrolidone hexanol solution, sodium citrate solution, graphene dispersion, anhydrous ethanol and aqueous ammonia were added in sequence, and stirred at a speed of 1000 r / min for 1 hour to obtain an emulsion; (2) adding tetraethoxysilane to the emulsion obtained in step (1), adjusting the temperature to 42° C., and stirring in a water bath for 2 hours to obtain a reaction solution; (3) centrifuging the reaction solution, filtering, washing, and drying to obtain a reaction material; (4) placing the reaction material in a resistance furnace, calcining it for 1 hour under the protection of an inert atmosphere, and then cooling it to room temperature to obtain a composite nano anti-wear agent.

3. The scratch-resistant and wear-resistant PP functional plastic according to claim 2, characterized in that: The mass fraction of the polyvinyl pyrrolidone hexanol solution in step (1) is 45%; The mass fraction of the graphene dispersion is 3.5%; The mass fraction of the sodium citrate solution is 10%; The mixing volume ratio of the polyvinyl pyrrolidone hexanol solution, the sodium citrate solution, the graphene dispersion, the anhydrous ethanol and the ammonia water is 80:3:5:10:

3.

4. The scratch-resistant and wear-resistant PP functional plastic according to claim 2, characterized in that: In step (2), the volume ratio of the emulsion to tetraethoxysilane is 5:

1.

5. The scratch-resistant and wear-resistant PP functional plastic according to claim 2, characterized in that: The centrifugal speed in step (3) is 6000 r / min, and the centrifugal time is 12 min; Washing is carried out by using anhydrous ethanol and deionized water in sequence, each washing for 10 minutes; The drying was performed at 65° C. for 10 hours.

6. The scratch-resistant and wear-resistant PP functional plastic according to claim 2, characterized in that: In step (4), the calcination temperature is 550-580° C. and the calcination time is 2 hours.

7. The scratch-resistant and wear-resistant PP functional plastic according to claim 2, characterized in that: In step (4), the inert atmosphere is either nitrogen or neon.

8. The scratch-resistant and wear-resistant PP functional plastic according to claim 1, characterized in that: The plasticizer is diisononyl phthalate; The stearate is magnesium stearate; The antioxidant is antioxidant 1010; The dispersant is glyceryl tristearate.

9. The scratch-resistant and wear-resistant PP functional plastic according to claim 1, characterized in that: The scratch-resistant and wear-resistant PP functional plastic is applied to a grater.

10. The method for preparing a scratch-resistant and wear-resistant PP functional plastic according to claim 1, characterized in that: The following steps are involved: S1 Preparation: Weigh the following according to weight: polypropylene resin, plasticizer, stearate, antioxidant, dispersant, composite nano anti-wear agent; S2 Mixing: Adding polypropylene resin, plasticizer, stearate, antioxidant, dispersant and composite nano anti-wear agent into a mixer in sequence, stirring and mixing to obtain a mixture; Among them, the stirring and mixing speed is 500r / min; The stirring time is 30 minutes; S3 Dry: The mixed material obtained in S2 is sent into a drying oven for drying, and after drying, a dry mixed material is obtained; Among them, the drying temperature is 80°C and the time is 1 hour; S4 Granulation: The dry mixed material is added into a twin-screw extruder for melt extrusion granulation to obtain the product.