High-resilience shoe insole material and forming method thereof
Through the extrusion granulation and supercritical foaming method of polyurethane mixture materials, high resilience shoe midsole materials are prepared, which solves the problems of poor rebound and insufficient high temperature resistance of traditional shoe materials and achieves higher resilience performance. and durability.
Patent Information
- Application Number
- CN202410790173.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional ultra-light EVA foam shoe materials have poor rebound, are prone to permanent deformation, and have poor high-temperature resistance, making it difficult to meet the performance requirements of high-quality sports shoes.
The polyurethane mixture material is extruded, granulated, and foamed. The composition includes thermoplastic polyurethane elastomer, polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, nylon elastomer, nucleating agent, Antioxidants and ultraviolet light absorbers are used to prepare high-rebound shoe midsole materials through supercritical foaming methods to improve their resilience and high-temperature aging resistance.
It significantly improves the resilience and high-temperature aging resistance of the midsole, prolongs its service life, and is suitable for the production of high-quality sports shoes.
Smart Images

Figure BDA0004899777630000091 
Figure BDA0004899777630000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane materials, in particular to a high-rebound shoe midsole material and a molding method thereof. Background Art
[0002] In the field of sports shoes, lighter shoes have an important impact on athletes' athletic performance and wearing experience, and lightweight materials have always been the pursuit of various brands. Traditionally, ultra-light ethylene-vinyl acetate copolymer (EVA) foam materials are used to make soles, which can meet the design requirements of ultra-light sports shoes. However, ultra-light EVA foam shoe materials have problems such as poor rebound and easy permanent deformation, making it difficult to meet the performance requirements of high-quality sports shoes.
[0003] Thermoplastic polyurethane elastomer (TPU) is a copolymer composed of hard segment and soft segment materials. It has the advantages of high tensile strength, high elongation, long-term compression and low permanent deformation rate. It is often used to manufacture higher quality sports shoes. At the same time, in order to enhance the performance of sports shoes, the current sole material preparation process uses foaming technology to foam TPU to obtain thermoplastic polyurethane elastomer foam material (ETPU). The soles prepared by ETPU can obtain higher resilience, deformation recovery and wear resistance, and its performance in all aspects far exceeds that of traditional EVA foam shoe materials.
[0004] However, ETPU still has the disadvantages of poor high temperature resistance and susceptibility to UV aging. Therefore, the present invention will improve ETPU with respect to these defects, and finally prepare a high-rebound shoe midsole material, which has certain practical significance. Summary of the invention
[0005] The object of the present invention is to provide a high-resilience shoe midsole material and a molding method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0007] A high-resilience shoe midsole material is prepared by extrusion granulation, foaming and molding of a polyurethane mixture; the polyurethane mixture comprises the following components, measured by weight: 50-60 parts of thermoplastic polyurethane elastomer, 5-10 parts of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 5-20 parts of nylon elastomer, 1-3 parts of nucleating agent, 0.2-0.5 parts of antioxidant and 0.2-1 parts of ultraviolet light absorber.
[0008] Furthermore, the molding method of the high-resilience shoe midsole material comprises the following steps:
[0009] Step 1: polyester polyol and diisocyanate react to generate polyurethane prepolymer, and then add modified fiber and ethylenediamine to prepare thermoplastic polyurethane elastomer;
[0010] Step 2: (1) mixing thermoplastic polyurethane elastomer, polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, nylon elastomer, nucleating agent, antioxidant and ultraviolet light absorber to obtain polyurethane mixture; (2) drying the polyurethane mixture, adding it into a twin-screw extruder for melt mixing, extruding and granulating to obtain polyurethane composite particles;
[0011] Step 3: After drying the polyurethane composite particles, a polyurethane foam material is prepared by a supercritical foaming method;
[0012] Step 4: injecting the polyurethane foam material into the shoe midsole mold of the water vapor molding machine, and finally preparing a high-resilience shoe midsole through steam heating, cold water cooling, drainage, and air cooling.
[0013] Furthermore, the preparation method of the thermoplastic polyurethane elastomer is as follows: (1) adding polyester polyol and stannous octoate into a reaction kettle, heating to 80-120°C, adjusting the pressure in the reaction kettle to be less than 500 Pa, and then adding diisocyanate to react for 1-3 hours to obtain a polyurethane prepolymer; (2) maintaining the original reaction temperature, adding modified fiber and ethylenediamine to the polyurethane prepolymer, mixing and stirring for 1-2 hours, casting into a mold at 100-120°C, and placing in an oven at 100-120°C for aging for 12-24 hours to obtain a thermoplastic polyurethane elastomer.
[0014] Furthermore, the thermoplastic polyurethane elastomer includes the following components, calculated by weight: 30-45 parts of polyester polyol, 20-30 parts of diisocyanate, 2-5 parts of modified fiber, 3-6 parts of ethylenediamine, and 0.03-0.05 parts of stannous octoate.
[0015] Furthermore, the diisocyanate includes, but is not limited to, one or more combinations of 4,4'-diphenylmethane diisocyanate, toluene diisocyanate, isophorone diisocyanate, p-phenylene diisocyanate, and 1,4-cyclohexane diisocyanate.
[0016] Furthermore, the preparation method of the polyester polyol is: phthalic anhydride, oxalic acid, 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, diethylene glycol, and stannous octoate are added to a reaction kettle, and the temperature is raised to 180-220° C. in a nitrogen environment, and the reaction is performed for 2-6 hours. During the reaction, if the detected acid value decreases to 20-30 mgKOH / g, vacuum dehydration is started, and the vacuum degree is maintained at -0.01 to -0.05 MPa until the acid value decreases to 1-3 mgKOH / g, then the reaction is stopped, and the polyester polyol is obtained after it is naturally cooled to room temperature.
[0017] Furthermore, the polyester polyol includes the following components, calculated by weight: 20-30 parts of phthalic anhydride, 10-15 parts of oxalic acid, 10-20 parts of 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, 10-20 parts of diethylene glycol, and 0.03-0.05 parts of stannous octoate.
[0018] Furthermore, the preparation method of the modified fiber is: adding hydroxyl-terminated polymethyl silicone oil, calcium carbonate whiskers, and carbon fibers to deionized water, ultrasonically dispersing for 5 to 15 minutes, heating to 50 to 70° C., stirring for 3 to 6 hours, and then filtering, washing, and drying to obtain the modified fiber.
[0019] Furthermore, the modified fiber includes the following components, calculated by weight: 7 to 10 parts of hydroxyl-terminated polymethyl silicone oil, 2 to 5 parts of calcium carbonate whiskers, and 1 to 3 parts of carbon fiber.
[0020] In the scheme, a polyester polyol was synthesized, which was prepared by condensation reaction of phthalic anhydride, oxalic acid, 4-4'-disulfadiylbis(4,1-phenylene)dimethanol and diethylene glycol. Phenyl groups and disulfide bonds were introduced to improve the high temperature resistance of thermoplastic polyurethane elastomer. Calcium carbonate whiskers and carbon fibers were further modified with hydroxyl-terminated polymethyl silicone oil to promote their dispersibility in the resin and increase their interfacial effect in the polyurethane prepolymer. Calcium carbonate whiskers mainly enhance the hardness of the thermoplastic polyurethane elastomer to ensure that it still has a strong hardness after foaming to meet the shoemaking needs of the foamed material. Carbon fibers mainly give the thermoplastic polyurethane elastomer high temperature aging resistance, and the two synergistically enhance the comprehensive performance of the thermoplastic polyurethane elastomer. In addition, the introduction of modified fibers can enhance the crosslinking density of the thermoplastic polyurethane elastomer, which can promote the subsequent foaming of the thermoplastic polyurethane elastomer, promote bubble growth and maintain stability.
[0021] Furthermore, the nucleating agent includes but is not limited to one or a combination of carbon black, talc, and mica.
[0022] Furthermore, the specific process of preparing the polyurethane composite particles is as follows: (1) placing the polyurethane mixture into a constant temperature dryer, setting the temperature at 60-80°C, and baking for 8-12 hours; (2) after baking, adding the polyurethane mixture into the barrel of a twin-screw extruder, melt-mixing at a temperature of 175-190°C and a rotation speed of 100-150 r / min, and finally extruding at a temperature of 170-180°C; (3) after extrusion, granulating at a rotation speed of 1500-2000 r / min through an underwater pelletizing system to obtain polyurethane composite particles.
[0023] In the scheme, in order to reduce the influence of subsequent foaming on the resilience of the polyurethane foam material, polystyrene-poly(ethylene-butylene)-polystyrene block copolymer and nylon elastomer are further added, wherein the polystyrene-poly(ethylene-butylene)-polystyrene block copolymer has excellent high temperature aging resistance, weather resistance and plasticity, and is well compounded with the thermoplastic polyurethane elastomer to improve the high temperature aging resistance of the thermoplastic polyurethane elastomer; the molecular chain structure of the nylon elastomer is equivalent to the polarity of the thermoplastic polyurethane elastomer, and the two can also be well compatible and compounded, and the nylon elastomer has excellent elasticity, so after compounding, it can support the growth and shaping of the polyurethane foam material bubbles and improve the shrinkage resistance of the bubbles; in addition, the amide group in the nylon elastomer can improve the high temperature resistance of the thermoplastic polyurethane elastomer.
[0024] Furthermore, the specific process of preparing the polyurethane foam material is as follows: (1) placing the polyurethane composite particles into a constant temperature dryer, setting the temperature at 60-80°C, and baking for 8-12 hours; (2) after baking, placing them into a high-pressure reactor, and introducing scCO2 into the high-pressure reactor until the foaming pressure is reached; (3) heating the high-pressure reactor to the foaming temperature under mechanical stirring, maintaining the temperature and pressure for 0.5-2 hours, and then quickly (<1s) releasing the pressure to normal pressure; (4) pressurizing the high-pressure reactor for a second time to the foaming pressure, repeating step (3), and placing it in a pressure-maintaining tank and maintaining the pressure for 24-48 hours to obtain the polyurethane foam material.
[0025] Furthermore, the foaming temperature is 80-120° C., and the foaming pressure is 10-20 MPa.
[0026] In the scheme, the polyurethane composite particles are foamed by supercritical foaming method to prepare polyurethane foam material; the supercritical foaming method can enhance the pore area of the polyurethane foam material, increase its foaming ratio, and then improve the resilience of the polyurethane foam material, reduce its hardness, and finally prepare the rebound performance of the midsole of the shoe better; in the specific implementation process, the foaming temperature, foaming pressure and pressure holding time have a decisive influence on the pore size of the polyurethane foam material. Generally speaking, the higher the foaming temperature and foaming pressure, the larger the pore structure obtained , and the longer the pressure and heat preservation time is, the smaller the shrinkage rate of the polyurethane foam material will be after the pressure is released, and the larger the pore structure will be. However, if the pore structure is too large, the prepared shoe midsole will be softer, and if it is too soft, the rebound resilience of the shoe midsole will be worse, making it easy for athletes to feel a sense of power loss during exercise, and the stability of the shoe will be poor, and it is easy to sprain the ankle. If the pore structure is too small, its rebound performance will be poor and the hardness will be high, and it is not suitable for processing into a shoe midsole. Therefore, the present invention needs to control the three factors to obtain a polyurethane foam material with a moderate pore structure.
[0027] Furthermore, the steam heating parameters are: heating temperature is 120-150° C., and heating time is 100-200 seconds.
[0028] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention prepares a thermoplastic polyurethane elastomer with excellent high temperature aging resistance and foaming promotion performance; through compounding with polystyrene-poly(ethylene-butylene)-polystyrene block copolymer and nylon elastomer, and subsequent control of foaming conditions, the pore structure of the thermoplastic polyurethane foam material is greatly improved, the foam material has excellent rebound performance and high temperature aging resistance, and can be made into a shoe midsole with high rebound and longer service life. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] It should be noted that the purchase manufacturers of all raw materials involved in the present invention are not subject to any special restrictions and exemplarily include: in the following embodiments: phthalic anhydride, oxalic acid, diethylene glycol, stannous octoate, toluene diisocyanate, isophorone diisocyanate, purity is 99%, purchased from Shanghai Jinjinle Industrial Co., Ltd.; 4-4'-disulfide dimethyl bis (4,1-phenylene) dimethanol purity 98%, CAS number: 7748-20-1, purchased from Tianshui Yiyao Chemical Co., Ltd.; hydroxyl-terminated polymethyl silicone oil molecular weight 1000~1 500, CAS No.: 156327-07-0, purchased from Shanghai Tangui New Materials Technology Co., Ltd.; calcium carbonate whisker purity 99.9%, length: 20-30 μm, diameter 1-2 μm, purchased from Shandong Jiaying Chemical Technology Co., Ltd.; carbon fiber model B-8110R, item No.: A1900, purchased from Dongguan Suyu Chemical Co., Ltd.; carbon black purity 99%, purchased from Hubei Shishun Biotechnology Co., Ltd.; polystyrene-poly(ethylene-butylene)-polystyrene block copolymer model KRATON G-1654, item No. 1654, purchased from Dongguan Dingxin Plastic Raw Materials Co., Ltd.; nylon elastomer model Pebax 7233, item No.: PEbax, purchased from Dongguan Jinshixiang Plastic Raw Materials Co., Ltd.; antioxidant model 412S, CAS No.: 3293-91-2, purchased from Tianjin Lianlong New Materials Co., Ltd.; ultraviolet light absorber purity 99%, model UV-360, purchased from Hubei Wande Chemical Co., Ltd.
[0031] Embodiment 1: A method for forming a high-resilience shoe midsole material:
[0032] Step 1: 1. Preparation of polyester polyol: 25 parts of phthalic anhydride, 12 parts of oxalic acid, 15 parts of 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, 15 parts of diethylene glycol, and 0.04 parts of stannous octoate are added to a reactor, heated to 200°C under a nitrogen environment, and reacted for 5 hours. During the reaction, if the detected acid value drops to 25 mgKOH / g, vacuum dehydration is started, and the vacuum degree is maintained at -0.01 MPa until the acid value drops to 2 mgKOH / g, then the reaction is stopped and allowed to cool naturally to room temperature to obtain polyester polyol;
[0033] 2. Preparation of modified fiber: 10 parts of hydroxyl-terminated polymethyl silicone oil, 4 parts of calcium carbonate whiskers, and 2 parts of carbon fiber were added to deionized water, ultrasonically dispersed for 10 minutes, heated to 60°C, stirred for reaction for 5 hours, filtered, washed, and dried to obtain modified fiber;
[0034] 3. The preparation method of thermoplastic polyurethane elastomer is as follows: (1) adding 40 parts of polyester polyol and 0.04 parts of stannous octoate into a reactor, heating to 100°C, adjusting the pressure in the reactor to less than 500 Pa, and then adding 10 parts of toluene diisocyanate and 15 parts of isophorone diisocyanate to react for 2 hours to obtain a polyurethane prepolymer; (2) maintaining the original reaction temperature, adding 4 parts of modified fiber and 4 parts of ethylenediamine into the polyurethane prepolymer, mixing and stirring for 2 hours, casting into a mold at 110°C, and placing in an oven at 110°C for aging for 24 hours to obtain a thermoplastic polyurethane elastomer;
[0035] Step 2: Preparation of polyurethane composite particles: (1) Put the polyurethane mixture (55 parts of thermoplastic polyurethane elastomer, 7 parts of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 15 parts of nylon elastomer, 2 parts of carbon black, 0.4 parts of 412S antioxidant, and 0.5 parts of UV-360 ultraviolet light absorber) into a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, add the polyurethane mixture into the barrel of a twin-screw extruder, melt-mix at a temperature of 180°C and a speed of 120 r / min, and finally extrude at a temperature of 175°C; (3) After extrusion, granulate at a speed of 1800 r / min through an underwater pelletizing system to obtain polyurethane composite particles;
[0036] Step 3: Preparation of polyurethane foam material: (1) Place the polyurethane composite particles in a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, place them in a high-pressure reactor, and introduce scCO2 into the high-pressure reactor until the foaming pressure (20Mpa) is reached; (3) Under mechanical stirring, heat the high-pressure reactor to the foaming temperature (110°C), keep the temperature and pressure for 1.5 hours, and then quickly (<1s) release the pressure to normal pressure; (4) Pressurize the high-pressure reactor again to the foaming pressure (20Mpa), repeat step (3), and place it in a pressure tank and keep the pressure for 48 hours to obtain a polyurethane foam material;
[0037] Step 4: Preparation of high-resilience shoe midsole: inject the polyurethane foam material into the shoe midsole mold of the steam molding machine, heat it to 140°C with steam, heat it for 150s, cool it with cold water, drain it, and cool it with air to finally prepare the high-resilience shoe midsole.
[0038] Embodiment 2: A method for forming a high-rebound shoe midsole material:
[0039] Step 1: 1. Preparation of polyester polyol: 25 parts of phthalic anhydride, 12 parts of oxalic acid, 10 parts of 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, 20 parts of diethylene glycol, and 0.04 parts of stannous octoate are added to a reactor, heated to 200°C under a nitrogen environment, and reacted for 5 hours. During the reaction, if the detected acid value drops to 25 mgKOH / g, vacuum dehydration is started, and the vacuum degree is maintained at -0.01 MPa until the acid value drops to 2 mgKOH / g, then the reaction is stopped and allowed to cool naturally to room temperature to obtain polyester polyol;
[0040] 2. Preparation of modified fiber: 7 parts of hydroxyl-terminated polymethyl silicone oil, 2 parts of calcium carbonate whiskers, and 1 part of carbon fiber were added to deionized water, ultrasonically dispersed for 10 minutes, heated to 60°C, stirred for reaction for 5 hours, filtered, washed, and dried to obtain modified fiber;
[0041] 3. The preparation method of thermoplastic polyurethane elastomer is as follows: (1) adding 40 parts of polyester polyol and 0.04 parts of stannous octoate into a reactor, heating to 100°C, adjusting the pressure in the reactor to less than 500 Pa, and then adding 10 parts of toluene diisocyanate and 15 parts of isophorone diisocyanate to react for 2 hours to obtain a polyurethane prepolymer; (2) maintaining the original reaction temperature, adding 4 parts of modified fiber and 4 parts of ethylenediamine into the polyurethane prepolymer, mixing and stirring for 2 hours, casting into a mold at 110°C, and placing in an oven at 110°C for aging for 24 hours to obtain a thermoplastic polyurethane elastomer;
[0042] Step 2: Preparation of polyurethane composite particles: (1) Put the polyurethane mixture (55 parts of thermoplastic polyurethane elastomer, 7 parts of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 15 parts of nylon elastomer, 2 parts of carbon black, 0.4 parts of 412S antioxidant, and 0.5 parts of UV-360 ultraviolet light absorber) into a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, add the polyurethane mixture into the barrel of a twin-screw extruder, melt-mix at a temperature of 180°C and a speed of 120 r / min, and finally extrude at a temperature of 175°C; (3) After extrusion, granulate at a speed of 1800 r / min through an underwater pelletizing system to obtain polyurethane composite particles;
[0043] Step 3: Preparation of polyurethane foam material: (1) Place the polyurethane composite particles in a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, place them in a high-pressure reactor, and introduce scCO2 into the high-pressure reactor until the foaming pressure (10Mpa) is reached; (3) Under mechanical stirring, heat the high-pressure reactor to the foaming temperature (100°C), keep the temperature and pressure for 0.5 hours, and then quickly (<1s) release the pressure to normal pressure; (4) Pressurize the high-pressure reactor again to the foaming pressure (10Mpa), repeat step (3), and place it in a pressure tank and keep the pressure for 24 hours to obtain a polyurethane foam material;
[0044] Step 4: Preparation of high-resilience shoe midsole: inject the polyurethane foam material into the shoe midsole mold of the steam molding machine, heat it to 140°C with steam, heat it for 150s, cool it with cold water, drain it, and cool it with air to finally prepare the high-resilience shoe midsole.
[0045] Embodiment 3: A method for forming a high-rebound shoe midsole material:
[0046] Step 1: 1. Preparation of polyester polyol: 25 parts of phthalic anhydride, 12 parts of oxalic acid, 20 parts of 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, 10 parts of diethylene glycol, and 0.04 parts of stannous octoate are added to a reactor, heated to 200°C under a nitrogen environment, and reacted for 5 hours. During the reaction, if the detected acid value drops to 25 mgKOH / g, vacuum dehydration is started, and the vacuum degree is maintained at -0.01 MPa until the acid value drops to 2 mgKOH / g, then the reaction is stopped and allowed to cool naturally to room temperature to obtain polyester polyol;
[0047] 2. Preparation of modified fiber: 10 parts of hydroxyl-terminated polymethyl silicone oil, 5 parts of calcium carbonate whiskers, and 3 parts of carbon fiber were added to deionized water, ultrasonically dispersed for 10 minutes, heated to 60°C, stirred for reaction for 5 hours, filtered, washed, and dried to obtain modified fiber;
[0048] 3. The preparation method of thermoplastic polyurethane elastomer is as follows: (1) adding 40 parts of polyester polyol and 0.04 parts of stannous octoate into a reactor, heating to 100°C, adjusting the pressure in the reactor to less than 500 Pa, and then adding 10 parts of toluene diisocyanate and 15 parts of isophorone diisocyanate to react for 2 hours to obtain a polyurethane prepolymer; (2) maintaining the original reaction temperature, adding 4 parts of modified fiber and 4 parts of ethylenediamine into the polyurethane prepolymer, mixing and stirring for 2 hours, casting into a mold at 110°C, and placing in an oven at 110°C for aging for 24 hours to obtain a thermoplastic polyurethane elastomer;
[0049] Step 2: Preparation of polyurethane composite particles: (1) Put the polyurethane mixture (55 parts of thermoplastic polyurethane elastomer, 7 parts of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 15 parts of nylon elastomer, 2 parts of carbon black, 0.4 parts of 412S antioxidant, and 0.5 parts of UV-360 ultraviolet light absorber) into a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, add the polyurethane mixture into the barrel of a twin-screw extruder, melt-mix at a temperature of 180°C and a speed of 120 r / min, and finally extrude at a temperature of 175°C; (3) After extrusion, granulate at a speed of 1800 r / min through an underwater pelletizing system to obtain polyurethane composite particles;
[0050] Step 3: Preparation of polyurethane foam material: (1) Place the polyurethane composite particles in a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, place them in a high-pressure reactor, and introduce scCO2 into the high-pressure reactor until the foaming pressure (20Mpa) is reached; (3) Under mechanical stirring, heat the high-pressure reactor to the foaming temperature (120°C), keep the temperature and pressure for 2 hours, and then quickly (<1s) release the pressure to normal pressure; (4) Pressurize the high-pressure reactor again to the foaming pressure (20Mpa), repeat step (3), and place it in a pressure tank and keep the pressure for 48 hours to obtain a polyurethane foam material;
[0051] Step 4: Preparation of high-resilience shoe midsole: inject the polyurethane foam material into the shoe midsole mold of the steam molding machine, heat it to 140°C with steam, heat it for 150s, cool it with cold water, drain it, and cool it with air to finally prepare the high-resilience shoe midsole.
[0052] Comparative Example 1: Comparative Example 1 is based on Example 1, and the amount of components of the polyurethane composite material is adjusted, and other processes remain unchanged, specifically:
[0053] Preparation of polyurethane composite particles: (1) Put a polyurethane mixture (61 parts of thermoplastic polyurethane elastomer, 1 part of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 15 parts of nylon elastomer, 2 parts of carbon black, 0.4 parts of 412S antioxidant, and 0.5 parts of UV-360 ultraviolet light absorber) into a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, add the polyurethane mixture into the barrel of a twin-screw extruder, melt-mix at a temperature of 180°C and a speed of 120 r / min, and finally extrude at a temperature of 175°C; (3) After extrusion, granulate at a speed of 1800 r / min through an underwater pelletizing system to obtain polyurethane composite particles.
[0054] Comparative Example 2: Comparative Example 2 is based on Example 1, and the amount of components of the polyurethane composite material is adjusted, and other processes remain unchanged, specifically:
[0055] Preparation of polyurethane composite particles: (1) Put a polyurethane mixture (69 parts of thermoplastic polyurethane elastomer, 7 parts of polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 1 part of nylon elastomer, 2 parts of carbon black, 0.4 parts of 412S antioxidant, and 0.5 parts of UV-360 ultraviolet light absorber) into a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, add the polyurethane mixture into the barrel of a twin-screw extruder, melt-mix at a temperature of 180°C and a speed of 120 r / min, and finally extrude at a temperature of 175°C; (3) After extrusion, granulate at a speed of 1800 r / min through an underwater pelletizing system to obtain polyurethane composite particles.
[0056] Comparative Example 3: Comparative Example 3 is based on Example 1, with the following adjustments: 4-4'-disulfadiylbis(4,1-phenylene)dimethanol is not added in the preparation of polyester polyol, and other processes remain unchanged, specifically:
[0057] Preparation of polyester polyol: 25 parts of phthalic anhydride, 12 parts of oxalic acid, 30 parts of diethylene glycol, and 0.04 parts of stannous octoate are added to a reactor, heated to 200°C under a nitrogen environment, and reacted for 5 hours. During the reaction, if the detected acid value drops to 25 mgKOH / g, vacuum dehydration is started and the vacuum degree is maintained at -0.01 MPa until the acid value drops to 2 mgKOH / g, then the reaction is stopped and it is allowed to cool naturally to room temperature to obtain polyester polyol.
[0058] Comparative Example 4: Comparative Example 4 is based on Example 1, with the following adjustments: no carbon fiber is added in the preparation of the modified fiber, and other processes remain unchanged, specifically:
[0059] Preparation of modified fiber: 10 parts of hydroxyl-terminated polymethyl silicone oil and 6 parts of calcium carbonate whiskers were added to deionized water, ultrasonically dispersed for 10 minutes, heated to 60°C, stirred for reaction for 5 hours, and then filtered, washed and dried to obtain modified fiber.
[0060] Comparative Example 5: Comparative Example 5 is based on Example 1, with the following adjustments: no modified fiber is added in the preparation of the thermoplastic polyurethane elastomer, and other processes remain unchanged, specifically:
[0061] The preparation method of thermoplastic polyurethane elastomer is as follows: (1) adding 40 parts of polyester polyol and 0.04 parts of stannous octoate into a reactor, heating to 100°C, adjusting the pressure in the reactor to be less than 500 Pa, and then adding 10 parts of toluene diisocyanate and 15 parts of isophorone diisocyanate to react for 2 hours to obtain a polyurethane prepolymer; (2) maintaining the original reaction temperature, adding 4 parts of ethylenediamine into the polyurethane prepolymer, mixing and stirring for 2 hours, casting into a mold at 110°C, and placing in an oven at 110°C for aging for 24 hours to obtain a thermoplastic polyurethane elastomer.
[0062] Comparative Example 6: Based on Example 1, Comparative Example 6 adjusted the following foaming parameters, while other processes remained unchanged, specifically:
[0063] Preparation of polyurethane foam material: (1) Place the polyurethane composite particles in a constant temperature dryer, set the temperature at 70°C, and bake for 10 hours; (2) After baking, place them in a high-pressure reactor, and introduce scCO2 into the high-pressure reactor until the foaming pressure (30Mpa) is reached; (3) Under mechanical stirring, heat the high-pressure reactor to the foaming temperature (130°C), keep the temperature and pressure for 2 hours, and then quickly (<1s) release the pressure to normal pressure; (4) Pressurize the high-pressure reactor again to the foaming pressure (30Mpa), repeat step (3), and place it in a pressure tank and keep the pressure for 48 hours to obtain a polyurethane foam material.
[0064] Performance test: The high-resilience shoe midsoles prepared in Examples 1 to 3 and Comparative Examples 1 to 6 were tested for performance respectively, and the specific test methods were as follows:
[0065] Test method: 1. According to the test standard of ASTM D2632-15, the rebound rate of the midsole of high rebound shoes is tested;
[0066] 2. According to the standard of GB / T 9640-2008, the high rebound shoe midsole was placed in a thermal oxygen aging test box, the temperature was set at 80°C, and the thermal oxygen aging was performed for 720 hours, and then the rebound rate test was performed; the test results of each group are shown in Table 1 below:
[0067] Table 1
[0068]
[0069]
[0070] Result analysis: From the data in Table 1 above, it can be seen that the present invention prepares a high-rebound shoe midsole with excellent heat resistance; the preparation of polyester polyols, modified fibers, thermoplastic polyurethane elastomers, the introduction of polystyrene-poly(ethylene-butylene)-polystyrene block copolymers, nylon elastomers, and the control of foaming parameters in the scheme all have a significant effect on the rebound performance of the shoe midsole.
[0071] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A high-rebound shoe midsole material, Features: The high-rebound shoe midsole material is prepared from a polyurethane mixture; the polyurethane mixture includes the following components, measured by weight: 50 to 60 parts of a thermoplastic polyurethane elastomer, 5 to 10 parts of a polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, 5 to 20 parts of a nylon elastomer, 1 to 3 parts of a nucleating agent, 0.2 to 0.5 parts of an antioxidant, and 0.2 to 1 parts of an ultraviolet light absorber.
2. A high-resilience shoe midsole material according to claim 1, Features: The preparation method of the thermoplastic polyurethane elastomer is: (1) adding polyester polyol and stannous octoate into a reaction kettle, heating the kettle to 80-120° C., adjusting the pressure in the reaction kettle to less than 500 Pa, and then adding diisocyanate to react for 1-3 hours to obtain a polyurethane prepolymer; (2) Maintaining the original reaction temperature, the modified fiber and ethylenediamine are added to the polyurethane prepolymer, mixed and stirred for 1 to 2 hours, and then cast into a mold at 100 to 120° C. and placed in an oven at 100 to 120° C. for aging for 12 to 24 hours to obtain a thermoplastic polyurethane elastomer.
3. A high-resilience shoe midsole material according to claim 2, Features: The thermoplastic polyurethane elastomer comprises the following components, calculated by weight: 30-45 parts of polyester polyol, 20-30 parts of diisocyanate, 2-5 parts of modified fiber, 3-6 parts of ethylenediamine, and 0.03-0.05 parts of stannous octoate.
4. A high-resilience shoe midsole material according to claim 2, Features: The preparation method of the polyester polyol is as follows: phthalic anhydride, oxalic acid, 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, diethylene glycol and stannous octoate are added into a reaction kettle, and the temperature is raised to 180-220° C. in a nitrogen environment, and the reaction is performed for 2-6 hours. During the reaction, if the detected acid value is reduced to 20-30 mgKOH / g, vacuum dehydration is started, and the vacuum degree is maintained at -0.01 to -0.05 MPa until the acid value is reduced to 1-3 mgKOH / g, then the reaction is stopped, and the polyester polyol is naturally cooled to room temperature to obtain the polyester polyol.
5. A high-resilience shoe midsole material according to claim 4, Features: The polyester polyol comprises the following components, calculated by weight: 20-30 parts of phthalic anhydride, 10-15 parts of oxalic acid, 10-20 parts of 4-4'-disulfadiylbis(4,1-phenylene)dimethanol, 10-20 parts of diethylene glycol, and 0.03-0.05 parts of stannous octoate.
6. A high-resilience shoe midsole material according to claim 2, Features: The preparation method of the modified fiber is as follows: hydroxyl-terminated polymethyl silicone oil, calcium carbonate whisker and carbon fiber are added to deionized water, ultrasonically dispersed for 5 to 15 minutes, heated to 50 to 70° C., stirred for reaction for 3 to 6 hours, filtered, washed and dried to obtain the modified fiber; The modified fiber includes the following components, calculated by weight: 7 to 10 parts of hydroxyl-terminated polymethyl silicone oil, 2 to 5 parts of calcium carbonate whiskers, and 1 to 3 parts of carbon fiber.
7. A method for forming a high-resilience shoe midsole material according to any one of claims 1 to 6, Features: The following steps are involved: Step 1: polyester polyol and diisocyanate react to generate polyurethane prepolymer, and then add modified fiber and ethylenediamine to prepare thermoplastic polyurethane elastomer; Step 2: (1) mixing thermoplastic polyurethane elastomer, polystyrene-poly(ethylene-butylene)-polystyrene block copolymer, nylon elastomer, nucleating agent, antioxidant and ultraviolet light absorber to obtain polyurethane mixture; (2) drying the polyurethane mixture, adding it into a twin-screw extruder for melt mixing, extruding and granulating to obtain polyurethane composite particles; Step 3: After drying the polyurethane composite particles, a polyurethane foam material is prepared by a supercritical foaming method; Step 4: injecting the polyurethane foam material into the shoe midsole mold of the water vapor molding machine, and finally preparing a high-resilience shoe midsole through steam heating, cold water cooling, drainage, and air cooling.
8. A method for forming a high-resilience shoe midsole material according to claim 7, Features: The specific process of preparing the polyurethane composite particles is as follows: (1) Place the polyurethane mixture into a constant temperature dryer, set the temperature at 60-80°C, and bake for 8-12 hours; (2) After baking, the polyurethane mixture is added into the barrel of a twin-screw extruder, melt-mixed at a temperature of 175 to 190° C. and a rotation speed of 100 to 150 r / min, and finally extruded at a temperature of 170 to 180° C.; (3) After extrusion, the polyurethane composite particles are obtained by pelletizing at a speed of 1500 to 2000 r / min through an underwater pelletizing system.
9. A method for forming a high-resilience shoe midsole material according to claim 7, Features: The specific process of preparing the polyurethane foam material is as follows: (1) placing the polyurethane composite particles into a constant temperature dryer, setting the temperature at 60 to 80° C., and baking for 8 to 12 hours; (2) After baking, it is placed in a high-pressure reactor, and scCO is introduced into the high-pressure reactor. 2 Until the foaming pressure reaches 10-20Mpa; (3) Under mechanical stirring, heat the autoclave to 80-120°C, maintain the temperature and pressure for 0.5-2h, and then quickly release the pressure to normal pressure; (4) The autoclave is pressurized for a second time to a foaming pressure, and step (3) is repeated, and the autoclave is placed in a pressure-maintaining tank and pressure-maintained for 24 to 48 hours to obtain a polyurethane foam material.
10. A method for forming a high-resilience shoe midsole material according to claim 7, Features: The steam heating parameters are as follows: heating temperature is 120-150° C., and heating time is 100-200 seconds.