Transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating

By constructing a micro-nano hierarchical structure on the surface of photovoltaic glass and regulating the island-like distribution of photocatalytic nanoparticles, the problem in the existing technology that the photocatalytic surface is difficult to be compatible with superhydrophobicity and photocatalysis is solved, and the transmittance antireflection, superhydrophobicity, and photocatalysis are achieved. Catalytic and wear-resistant self-cleaning coating suitable for room temperature curing and large-area applications of photovoltaic glass.

CN118755282AActive Publication Date: 2024-10-11XIAMEN UNIV

Patent Information

Application Number
CN202410736897.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-11
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

It is difficult to realize the compatibility of both superhydrophobic and photocatalytic functions on the surface of photovoltaic glass at the same time with the existing technology, resulting in the photocatalytic surface having photoinduced superhydrophilicity and being unable to be cured at room temperature, which limits its application scope.

Method used

By building a micro-nano hierarchical structure on the surface of the coating, mixing in photocatalytic nanoparticles, regulating its island-like distribution, and combining low surface energy modified hydrophobic SiO2 nanoparticles and coupling agents, a transparent superhydrophobic photocatalytic anti-reflective self-cleaning coating is formed. layer to achieve compatibility between superhydrophobicity and photocatalytic activity.

Benefits of technology

It achieves increased transmittance, has both super-hydrophobic and photocatalytic properties, has wear resistance, and can be cured at room temperature. It is suitable for large-area photovoltaic glass surfaces and is widely used in photovoltaics, construction, transportation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755282A_ABST
    Figure CN118755282A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of surface self-cleaning coatings, and particularly discloses a transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating which comprises a super-hydrophobic coating and a plurality of photocatalytic island-shaped areas distributed on the surface of the super-hydrophobic coating, and the photocatalytic island-shaped areas are formed by stacking photocatalytic nano-particles in a cluster mode. The super-hydrophobic coating comprises the following components: low surface energy modified hydrophobic SiO2 nanoparticles, silicate ester and a coupling agent, and the mass ratio of the photocatalytic nanoparticles to the hydrophobic SiO2 nanoparticles to the silicate ester to the coupling agent is (0.001-0.01): (0.05-0.1): 1: (1-5). The self-cleaning coating is prepared from photocatalytic nanoparticles, low-surface-energy-modified hydrophobic SiO2 nanoparticles, silicate ester, a coupling agent and the like through normal-temperature curing with a sol-gel method, a special surface structure is constructed, and the technical problem that photocatalysis and super-hydrophobicity are difficult to be compatible is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface self-cleaning coatings, and in particular relates to a transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating. Background Art

[0002] As people's demand for energy continues to increase, the application of photovoltaic panels and their components in independent and grid-connected modes is growing, especially in sunny areas, where large-scale photovoltaic power stations are becoming increasingly popular. However, photovoltaic modules are placed outdoors for a long time, and are prone to adsorb dust in the atmosphere and dust caused by traffic exhaust pollutants, causing dust to accumulate on the surface of photovoltaic glass, blocking the incidence of sunlight, resulting in a decrease in the transmittance of photovoltaic glass, and thus a decrease in photovoltaic efficiency. Therefore, in order to maintain power generation efficiency, solar panels need to be cleaned regularly every few weeks. At present, cleaning methods mainly include manual, semi-automatic, and automatic cleaning. Among them, manual cleaning methods and semi-automatic cleaning methods mainly include manual conventional cleaning, mechanical cleaning, and high-pressure water gun cleaning. These cleaning methods are time-consuming, costly, and harmful to the environment, and may even corrode the frame of the solar panel and damage the surface of the photovoltaic panel.

[0003] Self-cleaning coatings have natural self-cleaning capabilities, low energy consumption, environmental protection, and low maintenance. By constructing self-cleaning coatings on the surface of photovoltaic panels, the cleaning cycle of photovoltaic glass surfaces can be shortened, the frequency of surface cleaning can be reduced, and the power generation efficiency of photovoltaic modules can be maintained. At present, there are three main types of self-cleaning coatings: hydrophobic coatings, hydrophilic coatings, and photocatalytic coatings. The surfaces of hydrophobic coatings and hydrophilic coatings carry away dust and dirt in different ways through raindrops; photocatalytic coatings absorb ultraviolet light in sunlight through photocatalysts in the coatings to generate photogenerated electrons and photogenerated electron holes. Photogenerated electron holes have strong oxidation ability, and organic pollutants adsorbed on the surface of the coatings are oxidized and decomposed. The surface energy of hydrophilic coatings is in a high state and is easy to adsorb dust in the environment, while the surface energy of super-hydrophobic surfaces is low, and the dust deposition rate can be significantly reduced even without rainfall. Therefore, super-hydrophobic coatings have a wider range of applications and more advantages in self-cleaning. By constructing a super-hydrophobic photocatalytic coating, the photocatalytic powder on the surface of the coating can use sunlight to decompose organic pollutants that are not easily washed away by raindrops on the surface of photovoltaic glass. By weakening the interfacial bonding force between the organic pollutants and the surface of photovoltaic glass, the organic pollutants can be easily washed away by raindrops, thereby achieving self-cleaning of the photovoltaic glass surface.

[0004] At present, self-cleaning coatings are mainly superhydrophobic coatings or photocatalytic superhydrophilic coatings. The literature (JI Z, LIU Y, DU F. Rational design of superhydrophobic, transparent hybrid coating with superior durability [J]. Progress in Organic Coatings, 2021, 157) uses phenyltrimethoxy (PTMS), 1H, 1H, 2H, 2H-perfluorodialkyltrimethoxysilane (PFTS), 3-glycolyltrimethylol (GPTS), and trimethoxy (propyl) silane (TTPS) as raw materials to prepare a superhydrophobic self-cleaning coating by a sol-gel method, but the coating has no photocatalytic properties and cannot decompose organic pollutants on the surface of the coating. The document (CN 115625098 A) discloses a method for preparing a self-cleaning super-hydrophobic surface, wherein a fluorosilicone resin and an organic solvent are mixed, and hydrophobic nano-silica is added, and magnetic stirring and ultrasonic dispersion treatment are performed in sequence to obtain a hydrophobic sol solution. After spraying, the curing temperature is 60 to 90° C. to obtain a self-cleaning super-hydrophobic coating. However, the coating does not have the ability to photocatalytically decompose organic pollutants. Although the curing temperature is as low as 60 to 90° C., it still cannot be cured at room temperature, and its practical application is limited. Literature (BOUTAMART M, BRICHE S, NOUNEH K, et al. Transparent and self-cleaning surfaces based on nanocomposite sol-gel coatings [J]. Chemistry select, 2020, 5 (28): 8522-8531) uses tetraisopropyl titanate (TIPT) and tetraethyl orthosilicate (TEOS) as raw materials, and prepares a photocatalytic self-cleaning coating by sol-gel method and high-temperature thermal curing at 300°C-500°C for 2 hours. The coating becomes super-hydrophilic (photo-induced super-hydrophilic) under sunlight irradiation, but the coating cannot be super-hydrophobic. There are few studies on super-hydrophobic photocatalytic self-cleaning coatings. The technical difficulty is that the surface of the photocatalytic has a photo-induced super-hydrophilic property. Therefore, photocatalysis and super-hydrophobicity are difficult to be compatible, and it is difficult to integrate the two functions of super-hydrophobicity and photocatalysis on the same surface at the same time. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the prior art and provide a transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating, by constructing a micro-nano hierarchical structure on the surface of the coating, reducing the reflectivity of the coating and making the coating surface super-hydrophobic; mixing photocatalytic nanoparticles, regulating the surface morphology of the coating, making the photocatalytic nanoparticles distributed on the coating surface in the form of islands of micron-scale clusters, thereby making the super-hydrophobicity and photocatalytic activity compatible on the coating surface.

[0006] In order to achieve the above objectives, one of the technical solutions of the present invention is: a transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating, comprising a super-hydrophobic coating and a plurality of photocatalytic island regions distributed on the surface of the super-hydrophobic coating, wherein the photocatalytic island regions are formed by accumulation of photocatalytic nanoparticle clusters, and the components of the super-hydrophobic coating include low surface energy modified hydrophobic SiO2 nanoparticles, silicates and coupling agents, and the mass ratio of the photocatalytic nanoparticles, hydrophobic SiO2 nanoparticles, silicates and coupling agents is 0.001-0.01:0.05-0.1:1:1-5.

[0007] In a preferred embodiment of the present invention, it is characterized in that the photocatalytic nanoparticles are single semiconductor oxides or composite semiconductor oxides, the single semiconductor oxide is one of anatase TiO2, rutile TiO2, oxygen-deficient TiO2 and ZnO, and the composite semiconductor oxide is one of anatase / rutile mixed TiO2, metal-loaded / grafted / doped TiO2, non-metal-doped / grafted TiO2, and TiO2 / ZnO.

[0008] In a preferred embodiment of the present invention, the area diameter of the photocatalytic island region is 3-8 μm, the spacing between adjacent photocatalytic island regions is 10-100 μm, and the center spacing between adjacent photocatalytic island regions is 10-100 μm.

[0009] In a preferred embodiment of the present invention, when the photocatalytic island region is circular, its area diameter is the diameter of the circle; when the photocatalytic island region is non-circular, its area diameter is the diameter of the inscribed circle or circumscribed circle that contains 90% of the area of ​​the photocatalytic island region.

[0010] In a preferred embodiment of the present invention, the low surface energy modified hydrophobic SiO2 nanoparticles include nano-SiO2 particles modified with silane, fluorosilane or siloxane.

[0011] In a preferred embodiment of the present invention, the silicate is one of methyl orthosilicate, ethyl orthosilicate, trimethoxysilane, triethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane and diethyldiethoxysilane, and the coupling agent is one of silane coupling agents KH550, KH560 and KH570.

[0012] In a preferred embodiment of the present invention, the surface of the super-hydrophobic coating is a micro-nano hierarchical porous rough structure.

[0013] In order to achieve the above objectives, the second technical solution of the present invention is: a method for preparing a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating, comprising the following steps:

[0014] (1) mixing silicate, silane coupling agent, ethanol, isopropanol, and propylene glycol methyl ether in a mass ratio of 30-35:30-35:25-35:30-35:70-80 to obtain a sol A; mixing oxalic acid, 0.1 mol / L nitric acid, and water in a mass ratio of 0.5-1.0:120-140:15-25 to obtain a solution B; slowly adding the solution B to the sol A while stirring to obtain a sol C;

[0015] (2) mixing photocatalytic nanoparticles, low surface energy modified hydrophobic SiO2 nanoparticles, and silane coupling agent in a mass ratio of 0.03-0.15:1.5-2.5:65-75 to obtain a D sol;

[0016] (3) coating the C sol obtained in step (1) on the surface of the photovoltaic glass substrate, and then coating the D sol obtained in step (2) after curing at room temperature, and obtaining a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating after curing at room temperature.

[0017] Solution B is a catalyst for the hydrolysis of silicate, and sol C acts as a bonding layer.

[0018] During the spraying process, C sol and D sol cannot be mixed and sprayed together. C sol is sprayed first, and then D sol is sprayed. The purpose is that C sol is used as a bonding layer, and D sol is used as a functional layer for super hydrophobicity, photocatalysis and anti-reflection. After curing at room temperature, a part of the solidified layer of D sol is embedded in the solidified layer of C sol to improve the wear resistance of the functional layer against gravel impact. The method for improving the wear resistance of the functional layer is based on the principle of eventually making the functional layer half-embedded in the bonding layer. The method can be to increase the air pressure when spraying D sol, or shorten the distance between the spray gun and the substrate, or use mechanical pressing after spraying, so that the solidified layer of sol D is partially pressed into the bonding layer by pressure.

[0019] In a preferred embodiment of the present invention, the coating method in step (3) is one of spray coating, spin coating and scraper coating.

[0020] In a preferred embodiment of the present invention, the surface roughness Ra (ie, the mean roughness) of the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating is 10-100 nm.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The self-cleaning coating of the present invention has transmittance enhancement, and has both super-hydrophobic and photocatalytic properties, and the coating also has wear resistance;

[0023] 2. The self-cleaning coating of the present invention can be cured at room temperature and can be sprayed on the surface of large-area photovoltaic glass, so it can be widely used in photovoltaic, construction, transportation, electronics and other product fields;

[0024] 3. The self-cleaning coating of the present invention is prepared by curing at room temperature through a sol-gel method from photocatalytic nanoparticles, low surface energy modified hydrophobic SiO2 nanoparticles, silicates, coupling agents, etc., to construct a special surface structure, thus overcoming the technical difficulty of the incompatibility of photocatalysis and super-hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the structure of the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating of the present invention;

[0026] Figure 2 This is the EDX distribution diagram of Ti element spectrum on the coating surface prepared in Example 1;

[0027] Figure 3 This is the EDX distribution diagram of Ti element spectrum on the coating surface prepared in Example 2;

[0028] In the figure: 1-photocatalytic island area, 2-superhydrophobic coating, 3-photovoltaic glass substrate. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in more detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.

[0030] A transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating, such as Figure 1 As shown, it includes a super-hydrophobic coating and a plurality of photocatalytic island regions distributed on the surface of the super-hydrophobic coating, wherein the photocatalytic island regions are formed by accumulation of photocatalytic nanoparticle clusters, and the components of the super-hydrophobic coating include low surface energy modified hydrophobic SiO2 nanoparticles, silicate and coupling agent, and the mass ratio of the photocatalytic nanoparticles, hydrophobic SiO2 nanoparticles, silicate and coupling agent is 0.001-0.01:0.05-0.1:1:1-5.

[0031] The photocatalytic nanoparticles are single semiconductor oxides or composite semiconductor oxides, the single semiconductor oxide is one of anatase TiO2, rutile TiO2, oxygen-deficient TiO2 and ZnO, and the composite semiconductor oxide is one of anatase / rutile mixed TiO2, metal-loaded / grafted / doped TiO2, non-metal-doped / grafted TiO2, and TiO2 / ZnO.

[0032] The area diameter of the photocatalytic island region is 3-8 μm, the interval between the adjacent photocatalytic island regions is 10-100 μm, and the center distance between the adjacent photocatalytic island regions is 10-100 μm.

[0033] When the photocatalytic island region is circular, its area diameter is the diameter of the circle; when the photocatalytic island region is non-circular, its area diameter is the diameter of the inscribed circle or circumscribed circle containing 90% of the area of ​​the photocatalytic island region.

[0034] The diameter of a single photocatalytic island area is x ≥ 3μm. Because the organic pollutants floating in the air, mainly automobile exhaust and factory exhaust, fall on the surface of the coating, due to the high surface energy of the photocatalytic island area, in order to reduce the surface energy of the system, the organic pollutants floating in the air automatically fall on the photocatalytic island area with high surface energy. If the diameter of the photocatalytic island area is less than 3μm, the organic pollutants floating in the air with particles of 2.5μm or smaller can easily cover the entire photocatalytic island area, and it is difficult for sunlight to irradiate the photocatalytic island area. As a result, the organic pollutants are difficult to be decomposed by the photocatalytic island area, and the self-cleaning effect of the coating is poor. Therefore, the diameter of a single photocatalytic island area needs to meet x ≥ 3μm; the diameter of a single photocatalytic island area The diameter x≤8μm, because if the diameter of the photocatalytic island area is greater than 8μm, the photocatalytic island area will generate photogenerated electrons and photogenerated electron holes under sunlight. The photogenerated electron holes are highly oxidizing, oxidizing the oxygen ions in the TiO2 lattice and generating oxygen vacancies on the TiO2 surface, thereby causing the photocatalytic island area to become photo-superhydrophilic. When it rains, it is difficult for water droplets with particles of 8μm or larger to completely cover the island area. At this time, the water droplets falling on the photocatalytic island area are all within the photocatalytic island area, and therefore exhibit photo-induced superhydrophilicity, while the water droplets falling outside the photocatalytic island area are superhydrophobic, making the coating surface as a whole not superhydrophobic and having a poor self-cleaning effect. Therefore, the diameter of a single photocatalytic island area needs to satisfy x≤8μm.

[0035] There needs to be a gap between the photocatalytic island area and the surrounding adjacent photocatalytic island areas (the distance of the gap is denoted as z). If there is no gap, they will be connected together. Under sunlight irradiation, photoinduced superhydrophilicity, the photocatalysis of the coating is not compatible with superhydrophobicity, and the self-cleaning effect of the coating is poor; the center distance of adjacent photocatalytic island areas is y, y=x+z, where x and z satisfy 3≤x≤8 (μm), 10≤z≤100 (μm). If z≤10μm, the photocatalytic island areas are too dense, and the ratio of the area showing superhydrophobicity to the photocatalytic island areas showing photoinduced superhydrophilicity is small. Under sunlight irradiation, photoinduced superhydrophilicity, the photocatalysis of the coating is not compatible with superhydrophobicity, and the self-cleaning effect of the coating is poor. Conversely, if z≥100μm, the photocatalytic island areas are too few, and the coating has poor photocatalytic decomposition ability of organic pollutants. During long-term use, the organic pollutants on the surface of the coating gradually accumulate, causing the surface to gradually lose superhydrophobicity, ultimately resulting in poor self-cleaning effect. Therefore, z needs to satisfy 10≤z≤100 (μm).

[0036] When the shape of the photocatalytic island region is circular, the area diameter x is the diameter of the circle; when the shape of the photocatalytic island region is not circular, the diameter of its inscribed circle or circumscribed circle can be taken as the area diameter. When two adjacent photocatalytic island regions are of different sizes, their area diameters x1 and x2 can be taken respectively, and the distance between the centers of the two photocatalytic island regions is y, y = 1 / 2 (x1) + z + 1 / 2 (x2), where x1, x2 and z satisfy 3 ≤ x1 or x2 ≤ 8 (μm), 10 ≤ z ≤ 100 (μm)

[0037] The low surface energy modified hydrophobic SiO2 nanoparticles include nano SiO2 particles modified with silane, fluorosilane or siloxane.

[0038] The surface of the super-hydrophobic coating is a micro-nano hierarchical porous rough structure.

[0039] The silicate is one of methyl orthosilicate, ethyl orthosilicate, trimethoxysilane, triethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane and diethyldiethoxysilane, and the coupling agent is one of silane coupling agents KH550, KH560 and KH570.

[0040] A method for preparing a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating comprises the following steps:

[0041] (1) mixing silicate, silane coupling agent, ethanol, isopropanol, and propylene glycol methyl ether in a mass ratio of 30-35:30-35:25-35:30-35:70-80 to obtain a sol A; mixing oxalic acid, 0.1 mol / L nitric acid, and water in a mass ratio of 0.5-1.0:120-140:15-25 to obtain a solution B; slowly adding the solution B to the sol A while stirring to obtain a sol C;

[0042] (2) mixing photocatalytic nanoparticles, low surface energy modified hydrophobic SiO2 nanoparticles, and silane coupling agent in a mass ratio of 0.03-0.15:1.5-2.5:65-75 to obtain a D sol;

[0043] (3) coating the C sol obtained in step (1) on the surface of the photovoltaic glass substrate, and then coating the D sol obtained in step (2) after curing at room temperature, and obtaining a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating after curing at room temperature.

[0044] The coating method in step (3) is one of spray coating, spin coating and scraping coating.

[0045] The surface roughness Ra (i.e., the mean roughness value) of the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating obtained in the step (3) is 10-100 nm.

[0046] The photocatalytic island areas can be characterized by an electron microscope with an energy spectrometer; the micro-nano hierarchical porous rough structure constructed by hydrophobic SiO2 nanoparticles on the coating surface can be characterized by electron microscopy and atomic force microscopy.

[0047] First, the coating must meet the requirements of high transmittance and not affect the incidence of sunlight, that is, compared with the transmittance of the glass substrate, the transmittance of the glass surface after the coating of the present invention is applied is higher; secondly, it must have the requirements of hydrophobicity and photocatalytic activity to ensure that the coating can not only remove dust particles on the glass surface through water droplets, but also degrade organic stains through photocatalytic island areas; further, it must be resistant to gravel impact, that is, the interface bonding force between the coating and the glass must be strong and wear-resistant. Considering that photovoltaic power stations are usually set up in desert areas, the evaluation of wear resistance is based on resistance to gravel impact. Finally, in order to use it on a large scale on the surface of photovoltaic glass, it is necessary to prepare a coating that can be easily sprayed and can be cured at room temperature.

[0048] Example 1

[0049] A transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating, comprising a super-hydrophobic coating and a plurality of photocatalytic island regions formed by accumulation of photocatalytic nanoparticle clusters distributed on the surface of the super-hydrophobic coating, is prepared by the following method:

[0050] (1) 32 g of tetraethyl orthosilicate, 33 g of silane coupling agent KH560, 30 g of ethanol, 32 g of isopropanol, and 73 g of propylene glycol methyl ether were stirred at room temperature for 20 min to obtain sol A. 0.7 g of oxalic acid, 130 g of 0.1 mol / L nitric acid solution, and 20 g of water were stirred at room temperature for 20 min to obtain solution B. Solution B was slowly added to sol A while stirring, and stirred at room temperature for 2 h to obtain sol C.

[0051] (2) 2 g of hydrophobic gas-phase SiO2 nanopowder R972, 70 g of silane coupling agent KH560, and 0.032 g of photocatalytic nanopowder P25 (mixed crystal TiO2 nanopowder of anatase and rutile) were stirred at room temperature for 1 h to obtain sol D.

[0052] (3) A 300×300 mm low-iron sodium calcium silicon photovoltaic glass with components of SiO2 55 wt%, Al2O3 4 wt%, MgO 21 wt%, Na2O 15 wt%, CaO 1 wt%, and K2O 0.2 wt% was used as a substrate. The glass was cleaned and dried, and the C sol was sprayed on the glass surface at room temperature using a 1.0 mm caliber spray gun (W-101-101S) and an air pressure of 0.18-0.24 MPa. After drying for 15 minutes, the D sol was sprayed and dried for 10 hours to obtain a transparent super hydrophobic photocatalytic anti-reflection self-cleaning coating.

[0053] The UV-Vis-NIR spectrophotometer Lambda 750 produced by PerkinElmer Co., Ltd. was used to measure the transmission spectrum of the sample in the wavelength range of 250-2000nm, with a step size of 1nm. The surface and cross-sectional morphology of the sample were observed using a SU-70 scanning electron microscope (SEM) produced by Hitachi, Japan. The acceleration voltage was set to 5kV and combined with an energy dispersive X-ray spectrometer (EDX; Oxford INCA; 20kV) to characterize the element distribution on the surface, especially the element distribution of Ti. The water contact angle (WCA) of the sample surface was tested with a universal contact angle meter to characterize the hydrophobic performance. The Dimension Icon atomic force microscope (AFM) produced by Bruker was used to detect the nanomorphology of the sample surface and calculate the surface roughness. The wear resistance of the coating surface was tested by a rigorous gravel wear test, simulating the impact of daily outdoor dust on the photovoltaic glass surface. Gravel with a particle size of 500μm was used to simulate the dust in the daily environment. The sample was tilted about 40° and a funnel was fixed at a distance of about 15cm from the sample surface to the lower end of the funnel. The funnel was filled with gravel. Each 100g of gravel was an impact cycle, and 5 cycles of gravel impact tests were performed. The photocatalytic activity of the coating was characterized by the photocatalytic degradation of methylene blue (MB). The glass sample was placed in a 5mg / L MB solution and exposed to ultraviolet light (ultraviolet light intensity 365nm is 0.5mW / cm 2 ) After irradiation for 20min, 60min, and 100min, the absorbance of the solution at 665nm was measured accordingly, and a MB solution degradation rate change diagram and MB solution degradation kinetic curve were drawn after the coating was irradiated for 100min, and the rate constant of MB degradation was obtained, and the photocatalytic activity was evaluated using the rate constant. The photocatalytic island region structural characteristics and the self-cleaning coating performance results of the self-cleaning coating of this embodiment are shown in Table 1.

[0054] The transmittance of the glass substrate is 90.6%, and the transmittance of the self-cleaning coating obtained in Example 1 is 91.8%. After the coating is added to the surface of the glass substrate, the transmittance increases by 1.2% compared with the glass substrate. This result is due to the micro-nano hierarchical porous structure of the coating, and its roughness Ra is 42nm. When the Ra value is higher than 100nm, the surface is too rough, and it is easy to scatter light, which reduces the transmittance. On the contrary, when the Ra value is less than 10nm, the micro-nano hierarchical porous structure of the surface is not obvious, and the transmittance does not increase, but decreases.

[0055] The SEM observation of the coating surface is a micro-nano hierarchical porous structure. The average roughness Ra measured by atomic force microscopy is 42nm, which is in the range of 10nm≤Ra≤100nm, corresponding to the structure observed by the SEM. Figure 2This is the EDX distribution diagram of Ti element spectrum on the coating surface. Figure 2 The right picture in the figure is an enlarged view of the left picture; it can be seen that Figure 2 The Ti element clusters in the island area are piled up. Figure 2 The small yellow bright spots dispersed in the middle are the background of the EDX test; it can be seen that the diameter of the photocatalytic island area of ​​the photocatalytic nanoparticle coating is x = 4μm, the interval between the adjacent photocatalytic island areas is z = 72μm, x and z meet the requirements of 3≤x≤8(μm), 10≤z≤100(μm), and the center distance between adjacent photocatalytic island areas is y, y=x+z=78μm, therefore, the water contact angle of the coating reaches 153°, achieving super hydrophobicity, and the rate constant of photocatalytic decomposition of methylene blue MB reaches 0.0055min -1 , has the ability to photocatalytically decompose organic pollutants.

[0056] The coating is exposed to ultraviolet light at 365nm and 1mW / cm 2 After 24 hours of irradiation, the water contact angle of the coating was 152°, which was very small compared to the initial 153°, and the coating surface still showed super hydrophobic properties. Since the coating meets the structural characteristics of the area diameter x of the photocatalytic island area and the interval z between the adjacent photocatalytic island areas, and x and z meet 3≤x≤8(μm), 10≤z≤100(μm), even under ultraviolet light irradiation, the coating surface will not lose its super hydrophobic properties due to the photoinduced super hydrophilicity of the photocatalytic island area.

[0057] After 5 gravel impact tests with 100g of grit each time, the water contact angle of the coating still reached 136°, showing excellent wear resistance.

[0058] In summary, the self-cleaning coating obtained in Example 1 has the structural characteristics that the area diameter x of the photocatalytic island region and the spacing z between adjacent photocatalytic island regions respectively meet the requirements of 3≤x≤8 (μm) and 10≤z≤100 (μm), and the surface roughness (roughness mean Ra) is in the range of 10nm≤Ra≤100nm. Therefore, the coating has transmittance enhancement, super hydrophobic properties and photocatalytic properties, and the coating also has wear resistance.

[0059] Example 2

[0060] A transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating, comprising a super-hydrophobic coating and a plurality of photocatalytic island regions formed by the accumulation of photocatalytic nanoparticle clusters distributed on the surface of the super-hydrophobic coating, the preparation method is the same as that of Example 1, and the difference from Example 1 is that the weight of the photocatalytic nanopowder P25 (anatase and rutile mixed crystal TiO2 nanopowder) is changed from 0.032g to 0.15g, and the rest is the same as Example 1. The structural characteristics of the photocatalytic island regions and the coating properties of the self-cleaning coating obtained in this embodiment are shown in Table 1.

[0061] The EDX distribution diagram of Ti element on the surface of the self-cleaning coating obtained in Example 2 is as follows: Figure 3 As shown, it can be seen, Figure 3 The Ti element clusters in the island area are piled up. Figure 3 The small yellow bright spots scattered in the middle are the background of the EDX test; it can be seen that the area diameter of the photocatalytic island region of the photocatalytic nanoparticle coating is x=8μm, the spacing between the surrounding adjacent photocatalytic island regions is z=10μm, and the center distance between adjacent photocatalytic island regions is y, y=x+z=18μm. Its structural characteristics are that the area diameter x of the photocatalytic island region and the spacing z between the surrounding adjacent photocatalytic island regions, x and z meet the requirements of 3≤x≤8(μm), 10≤z≤100(μm), and the surface roughness (roughness mean Ra) is in the range of 10nm≤Ra≤100nm. Therefore, the coating has transmittance enhancement, and the superhydrophobic property is compatible with the photocatalytic property, and has both superhydrophobic and photocatalytic properties; the coating also has wear resistance.

[0062] Comparative Example 1

[0063] A transparent super-hydrophobic photocatalytic anti-reflection self-cleaning coating, the preparation method is the same as that of Example 1, and the difference from Example 1 is that the weight of the photocatalytic nanopowder P25 (anatase and rutile mixed crystal TiO2 nanopowder) is changed from 0.032g to 0.0g, that is, during the coating preparation process, no photocatalytic nanoparticles are added, and the rest is the same as Example 1. The photocatalytic island region structural characteristics and coating properties of the obtained self-cleaning coating are shown in Table 1 below.

[0064] The coating obtained in Comparative Example 1 has the structural characteristics of having no photocatalytic island areas, and does not meet the requirements of the area diameter x of the photocatalytic island areas and the spacing z between the surrounding adjacent photocatalytic island areas, 3≤x≤8 (μm), 10≤z≤100 (μm). Although the surface roughness (roughness mean Ra) is in the range of 10nm≤Ra≤100nm, the coating has transmittance enhancement but no photocatalytic performance. It has certain superhydrophobic properties, and the water contact angle is much lower than that of Example 1 and Example 2, and cannot have both superhydrophobic and photocatalytic properties.

[0065] Comparative Example 2

[0066] A transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating, the preparation method is the same as that of Example 1, the difference from Example 1 is that the weight of the photocatalytic nanopowder P25 (anatase and rutile mixed crystal TiO2 nanopowder) is changed from 0.032g to 1.5g, and the rest is the same as Example 1.

[0067] The surface photocatalytic island region structural characteristics and coating performance of the self-cleaning coating obtained in Comparative Example 2 are shown in Table 1 below.

[0068] The coating obtained in Comparative Example 2, although there are photocatalytic island regions, the photocatalytic island regions are large in area, and the interval between adjacent photocatalytic island regions is 5 μm, which is very narrow. Due to the photoinduced superhydrophilic reaction of the photocatalytic island regions, the water contact angle is 118°, there is no superhydrophobicity, and the transmittance is lower than that of the substrate. Its structural characteristics are that the photocatalytic island regions do not meet the requirements of the area diameter x of the photocatalytic island regions and the interval z of the surrounding adjacent photocatalytic island regions, 3≤x≤8 (μm), 10≤z≤100 (μm), although the surface roughness (roughness mean Ra) is in the range of 10nm≤Ra≤100nm, therefore, the coating obtained in Comparative Example 2 cannot have both superhydrophobicity and photocatalytic properties.

[0069] Comparative Example 3

[0070] The weight of the photocatalytic nanopowder P25 (mixed crystal TiO2 nanopowder of anatase and rutile) was changed from 0.032g in Example 1 to 3.0g, and the hydrophobic gas-phase SiO2 nanopowder R972 was changed from 2g in Example 1 to 0g, that is, no hydrophobic SiO2 nanoparticles were added during the coating preparation process. The rest was the same as Example 1.

[0071] The surface photocatalytic island region structural characteristics and coating properties of the self-cleaning coating obtained in Comparative Example 3 are shown in Table 1 below.

[0072] The coating obtained in Comparative Example 3 has a photocatalytic area on the surface, which is connected into one piece, and there is no photocatalytic island area. Due to the photocatalytic photoinduced superhydrophilic reaction, the water contact angle is 46°, the coating is hydrophilic, not hydrophobic, and the transmittance is lower than that of the substrate. Its structure does not meet the requirements of the diameter x of the photocatalytic island area, the spacing z of the adjacent photocatalytic island areas, 3≤x≤8 (μm), 10≤z≤100 (μm), although the surface roughness (roughness mean Ra) is in the range of 10nm≤Ra≤100nm, therefore, the coating obtained in Comparative Example 3 cannot have both superhydrophobic and photocatalytic properties.

[0073] Table 1 Photocatalytic island region structural characteristics and coating properties of self-cleaning coatings obtained in Examples 1-2 and Comparative Examples 1-3

[0074]

[0075]

[0076] Note: The diameter of the photocatalytic island area is x (μm); the distance between the centers of the adjacent photocatalytic island areas is y, and the interval between the adjacent photocatalytic island areas is z, y=x+z.

[0077] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating, It is characterized in that The invention comprises a super hydrophobic coating and a plurality of photocatalytic island regions distributed on the surface of the super hydrophobic coating, wherein the photocatalytic island regions are formed by the accumulation of photocatalytic nanoparticle clusters, and the components of the super hydrophobic coating include hydrophobic SiO modified with low surface energy. 2 Nanoparticles, silicate and coupling agent, the photocatalytic nanoparticles, hydrophobic SiO 2 The mass ratio of nanoparticles, silicate and coupling agent is 0.001-0.01:0.05-0.1:1:1-5.

2. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 1, It is characterized in that The photocatalytic nanoparticles are single semiconductor oxides or composite semiconductor oxides, and the single semiconductor oxide is anatase TiO 2 , rutile TiO 2 、Oxygen-deficient TiO 2 and one of ZnO, the composite semiconductor oxide anatase / rutile mixed type TiO 2 , Metal-loaded / grafted / doped TiO 2 , Non-metal doped / grafted TiO 2 、TiO 2 / One of ZnO.

3. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 1, It is characterized in that The area diameter of the photocatalytic island region is 3-8 μm, the interval between the adjacent photocatalytic island regions is 10-100 μm, and the center distance between the adjacent photocatalytic island regions is 10-100 μm.

4. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 3, It is characterized in that When the photocatalytic island region is circular, its area diameter is the diameter of the circle; when the photocatalytic island region is non-circular, its area diameter is the diameter of the inscribed circle or circumscribed circle containing 90% of the area of ​​the photocatalytic island region.

5. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 1, It is characterized in that The low surface energy modified hydrophobic SiO 2 Nanoparticles include silane or fluorosilane or siloxane modified nano-SiO 2 Particles.

6. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 1, It is characterized in that The silicate is one of methyl orthosilicate, ethyl orthosilicate, trimethoxysilane, triethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diethyldimethoxysilane and diethyldiethoxysilane, and the coupling agent is one of silane coupling agents KH550, KH560 and KH570.

7. The transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 1, It is characterized in that The surface of the super hydrophobic coating is a micro-nano graded porous rough structure.

8. A method for preparing a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) mixing silicate, silane coupling agent, ethanol, isopropanol, and propylene glycol methyl ether in a mass ratio of 30-35:30-35:25-35:30-35:70-80 to obtain a sol A; mixing oxalic acid, 0.1 mol / L nitric acid, and water in a mass ratio of 0.5-1.0:120-140:15-25 to obtain a solution B; slowly adding the solution B to the sol A while stirring to obtain a sol C; (2) Photocatalytic nanoparticles and low surface energy modified hydrophobic SiO 2 The nanoparticles and the silane coupling agent are mixed and stirred in a mass ratio of 0.03-0.15:1.5-2.5:65-75 to obtain a D sol; (3) coating the C sol obtained in step (1) on the surface of the photovoltaic glass substrate, and then coating the D sol obtained in step (2) after curing at room temperature, and obtaining a transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating after curing at room temperature.

9. The method for preparing the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 8, It is characterized in that The coating method in step (3) is one of spray coating, spin coating and scraping coating.

10. The method for preparing the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating according to claim 8, It is characterized in that The surface roughness Ra of the transparent super-hydrophobic photocatalytic anti-reflective self-cleaning coating obtained in the step (3) is 10-100 nm.

Citation Information

Patent Citations

  • Preparation method of self-cleaning super-hydrophobic surface

    CN115625098A

  • Precoated steel sheet and process for producing same

    CN102574363A

  • Anti-reflection super-hydrophobic self-cleaning SiO2 nano coating

    CN105565678A

  • Preparation method and application of transparent super-hydrophobic super-oleophobic SiO2 nanometer functional liquid

    CN109181536A

  • Self-cleaning coating with super-hydrophobic and photocatalytic functions and preparation method thereof

    CN114574086A

Cited By

  • Polarizer and display device

    CN119846763A