Intumescent reinforced anti-cracking fireproof coating for steel structure

By using phosphorylated POSS-based flame retardants to graft modified chopped fibers and intumescent flame retardants to modify UiO-66 hybrid nanomaterials in steel structure fire retardant coatings, the poor thermal insulation performance and easy cracking of traditional intumescent fire retardant coatings are solved solve the problem and achieve efficient flame retardant and fire protection performance improvement.

CN118755296AActive Publication Date: 2024-10-11JIANGNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410815763.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11
Estimated Expiration
2044-06-24

AI Technical Summary

Technical Problem

Traditional intumescent fire retardant coatings are difficult to foam evenly on the surface of steel structural materials. The carbon layer formed has poor thermal insulation properties and is prone to cracking. It cannot effectively protect steel structural materials, resulting in reduced fire resistance.

Method used

Phosphorylated POSS-based flame retardants are used to graft modified chopped fibers and intumescent flame retardants to modify UiO-66 hybrid nanomaterials to form an intumescent steel structure fire retardant coating that enhances anti-cracking and improves thermal insulation performance and anti-cracking problems.

Benefits of technology

Significantly improves the flame retardant performance and fire safety performance of steel structure fire retardant coatings, ensuring the stability and fire protection performance of steel structure materials at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755296A_ABST
    Figure CN118755296A_ABST
Patent Text Reader

Abstract

The invention discloses an intumescent reinforced anti-cracking fireproof coating for a steel structure, and belongs to the technical field of intumescent fireproof coatings. The preparation method of the coating comprises the following steps: 1, preparing the phosphorylated POSS-based flame retardant grafted modified chopped fibers; 2, preparing a UiO-66 hybrid nano material loaded with an intumescent flame-retardant coating; and 3, preparation of the intumescent and enhanced anti-cracking fireproof coating for the steel structure added with the flame-retardant chopped fibers and the modified UiO-66. According to the invention, the phosphorylated POSS-based flame retardant grafted modified chopped fibers are introduced into an intumescent flame-retardant system loaded with an intumescent flame-retardant coating UiO-66 nano material, so that the cracking of the steel structure intumescent fireproof coating is effectively prevented, the expansion of a carbon layer is promoted, the strength of the carbon layer is improved, the heat resistance, the char forming performance and the flame-retardant performance of a matrix are synergistically and efficiently improved, and the preparation method is simple and efficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of intumescent fire-retardant coatings, in particular to an intumescent, enhanced anti-cracking steel structure fire-retardant coating. Background Art

[0002] Steel structure building materials are widely used in airports, stadiums, industrial plants and other construction fields due to their light weight, high strength, excellent seismic performance, simple construction, strong designability and environmental friendliness. Steel structure materials themselves are not easy to burn, but they are very easy to conduct heat, and their mechanical strength will gradually decrease with the increase of temperature. When the temperature exceeds 500℃, the mechanical strength of steel structure materials will drop sharply until they lose their supporting function, causing the building to collapse. However, when a fire occurs, the fire temperature can reach more than 700℃ in a short time, which means that steel structure building materials used in large quantities are at risk of damage in a very short time. According to the survey, in actual application, the fire resistance limit of exposed steel structure materials is only about 15 minutes, which greatly increases the difficulty of firefighting and rescue. In order to increase the time of fire rescue, reduce casualties and reduce economic and property losses, using fire retardant coatings on the surface of steel structure materials to improve their fire resistance limit is a simple, effective and economical means of safe fire prevention.

[0003] Constructing a fire-retardant coating on the surface of steel structure materials to make it fireproof and heat-insulating can further prevent its mechanical strength from decreasing significantly and causing the building to collapse. Fire-retardant coatings are divided into intumescent fire-retardant coatings and non-intumescent fire-retardant coatings. Among them, intumescent fire-retardant coatings are widely used in fire-retardant applications of steel structure materials due to their excellent flame retardant properties, economical and practical, and simple operation. Traditional intumescent coatings are generally composed of three parts: dehydrating agent, carbonizing agent and foaming agent. They contain a large amount of phosphorus and nitrogen elements, which play a synergistic flame retardant role. When the intumescent fire-retardant coating is heated, the dehydrating agent decomposes to release inorganic acids such as phosphoric acid, which promotes the dehydration of the carbonizing agent and the polymer matrix to form coke; the foaming agent decomposes to produce ammonia, water vapor and other flame-retardant and non-toxic gases, which take away the heat of the matrix and expand the molten carbon layer to form a foam-like structure. Therefore, the intumescent carbon layer formed on the surface of the steel structure material is heat-insulating and oxygen-insulating, which can effectively prevent the substrate from heating up and play a role in fire retardant of the building.

[0004] Intumescent fire-retardant coatings have the problem of being difficult to foam evenly, and are not easy to form a carbon layer or the formed carbon layer has poor thermal insulation performance, which affects its fire resistance and cannot effectively protect the steel structure base material. In addition, there is also the problem that the coating is easy to crack and cannot prevent corrosion from external media, causing the coating to fall off, thereby reducing its fire resistance or losing its fireproof effect. Therefore, it is necessary to develop an intumescent fire-retardant coating with good flame retardant properties, uniform foaming and not easy to crack. Summary of the invention

[0005] In order to solve the above problems, the present invention utilizes phosphorylated POSS-based flame retardant to graft-modify short-cut fibers, and adds them to the intumescent flame retardant modified UiO-66 hybrid nanomaterial intumescent fire retardant coating, so as to help improve the problems of poor carbonization and thermal insulation performance and easy cracking of traditional intumescent fire retardant coatings, and construct an enhanced intumescent steel structure fire retardant coating with integrated smoke suppression, toxicity reduction, high efficiency flame retardancy and anti-cracking.

[0006] A first aspect of the present invention provides a method for preparing a flame retardant modified chopped carbon fiber material, comprising the following steps:

[0007] 1. Synthesis of A-POSS solid: 3-aminopropyltriethoxysilane is dissolved in anhydrous methanol solution, mixed with hydrochloric acid solution, allowed to react for a period of time, and after solid-liquid separation, the obtained product is A-POSS solid;

[0008] 2. Preparation of phosphorylated POSS-based flame retardant grafted modified chopped fibers: dissolve the A-POSS solid obtained in step 1 in water, heat to 45-50°C, add formaldehyde, stir thoroughly for 30-40 minutes, then heat to 55-60°C, add phosphorous acid, after the solution is clarified, add chopped carbon fibers, heat to 85-95°C, stir to react, separate the solid and liquid and dry, the obtained fiber material is the flame retardant modified chopped carbon fiber material.

[0009] Furthermore, in step 1, the volume ratio of 3-aminopropyltriethoxysilane to anhydrous methanol is 1:7.8 to 1:10.

[0010] Furthermore, the mass concentration of the hydrochloric acid solution in step 1 is 30-40%.

[0011] Furthermore, in step 1, the ratio of 3-aminopropyltriethoxysilane to the hydrochloric acid solution is 1:1.4 to 1:2.

[0012] Furthermore, the mixing time in step 1 is 1 to 5 days.

[0013] Furthermore, the static reaction time in step 1 is 1 to 10 days.

[0014] Furthermore, the mass ratio of the A-POSS solid to water in step 2 is 1:100 to 20:100.

[0015] Furthermore, the molar ratio of NH bonds to formaldehyde in the A-POSS solid in step 2 is 1:16 to 1:32.

[0016] Furthermore, the molar ratio of NH bonds to phosphorous acid in the A-POSS solid in step 2 is 1:16 to 1:32.

[0017] Furthermore, in step 2, the mass ratio of the A-POSS solid to the formaldehyde solution is 1:5 to 1:10.

[0018] Furthermore, in step 2, the mass ratio of A-POSS solid to phosphorous acid is 1:1 to 1:2.

[0019] Furthermore, the length of the chopped carbon fiber in step 2 is 0.1 to 10 mm.

[0020] Furthermore, the stirring reaction time in step 2 is 8 to 12 hours.

[0021] The invention provides a flame retardant modified short-cut carbon fiber material prepared according to the method.

[0022] The second aspect of the present invention provides a method for preparing a UiO-66 hybrid nanomaterial loaded with an intumescent flame retardant coating, comprising the following steps:

[0023] S1. Preparation of UiO-66 micro-nano material: dissolving the transition metal salt compound and the organic ligand in a solvent respectively and mixing them evenly, reacting them under a certain temperature condition to obtain a suspension; collecting the suspension by centrifugation to precipitate, washing it with methanol or water for multiple times, and finally drying the obtained solid to obtain the product, which is the UiO-66 micro-nano material;

[0024] S2. Preparation of flame retardant modified solution: dissolving chitosan in a solvent to prepare a chitosan solution of a certain concentration; dissolving ammonium polyphosphate in a solvent to prepare an ammonium polyphosphate solution of a certain concentration;

[0025] S3. Preparation of UiO-66 hybrid nanomaterials loaded with intumescent flame retardant coating:

[0026] a. Immersing the UiO-66 micro-nano material obtained in step S1 in the chitosan solution in step S2, and then collecting and washing the particle precipitate to remove the unadsorbed chitosan particles;

[0027] b. Immersing the particle precipitate obtained in step a in the prepared ammonium polyphosphate solution, collecting the particle precipitate after a certain period of time and washing it to remove the unabsorbed ammonium polyphosphate particles, thus completing the expansion flame retardant modification of the UiO-66 nanomaterial;

[0028] c. Repeat steps a to b 3 to 10 times.

[0029] Furthermore, the transition metal salt compound in step S1 is one or more of metal zirconium salts such as zirconium chloride, zirconium sulfate, and zirconium acetate.

[0030] Furthermore, the organic ligand described in step S1 is one or more of terephthalic acid, trimesic acid and dimethylimidazole.

[0031] Furthermore, the solvent in step S1 is one or more of water, methanol, anhydrous ethanol and N,N-dimethylformamide.

[0032] Furthermore, the concentration of the transition metal salt compound in the suspension in step S1 is 0.01 to 0.05 mol / L.

[0033] Furthermore, the concentration of the organic ligand in the suspension in step S1 is 0.01-0.05 mol / L.

[0034] Furthermore, the certain temperature in step S1 is 100-180°C.

[0035] Furthermore, the reaction time in step S1 is 10 to 48 hours.

[0036] Furthermore, the centrifugal speed in step S1 is 1000-9000 r / min, and the centrifugal time is 3-10 min.

[0037] Furthermore, the drying temperature in step S1 is 45 to 120° C., and the drying time is 1 to 8 hours.

[0038] Furthermore, the solvent in step S2 is one or more of water, acetic acid, and N,N-dimethylformamide.

[0039] Furthermore, the chitosan solution in step S2 has a concentration of 0.5-5 wt%.

[0040] Furthermore, the concentration of the ammonium polyphosphate solution in step S2 is 0.5-5wt%.

[0041] Furthermore, in step S3, the soaking time in step a and step b is 1 to 10 minutes.

[0042] The invention provides a UiO-66 hybrid nano material loaded with an expansion flame retardant coating prepared according to the method.

[0043] The third aspect of the present invention provides a method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating, comprising the following steps:

[0044] Ⅰ. Preparation of base material: weigh the film former and curing agent and stir until a uniformly mixed base material is obtained;

[0045] Ⅱ. Preparation of intumescent, enhanced anti-cracking fire retardant coating for steel structure: Take the base material and the UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, mix and stir to form a uniform dispersion system; then, add the flame retardant modified chopped carbon fiber material to the uniform dispersion system and disperse it evenly to obtain the intumescent, enhanced anti-cracking fire retardant coating for steel structure.

[0046] Furthermore, the film-forming agent in step I includes one or more of epoxy resin, polyurethane, acrylic acid, and water-based silicone acrylic emulsion.

[0047] Furthermore, the curing agent in step I includes one or a combination of ethylenediamine, diethylenetriamine, triethylenetetramine, and 4,4-diaminodiphenylmethane.

[0048] Furthermore, in step I, the ratio of the film-forming agent to the curing agent is 1.5:1 to 5:1.

[0049] Furthermore, in step II, the base material accounts for 92.0-99.0% of the total weight of the uniformly dispersed system.

[0050] Furthermore, in step II, the UiO-66 hybrid nanomaterial loaded with the intumescent flame retardant coating accounts for 1 to 8.0% of the total weight of the uniformly dispersed system.

[0051] Preferably, the UiO-66 hybrid nanomaterial loaded with the intumescent flame retardant coating in step II accounts for 1 to 2.0% of the total weight of the uniformly dispersed system.

[0052] Furthermore, in step II, the flame retardant modified chopped carbon fiber material accounts for 0.5-10% of the uniformly dispersed system.

[0053] Preferably, the flame retardant modified chopped carbon fiber material in step II accounts for 0.8-1.2% of the uniformly dispersed system.

[0054] The present invention provides an intumescent, enhanced anti-cracking steel structure fire retardant coating prepared according to the method.

[0055] The invention provides an application of an intumescent, enhanced anti-cracking steel structure fire retardant coating in the field of fire prevention and fire retardant product preparation.

[0056] Furthermore, the application comprises the following steps:

[0057] The intumescent, enhanced anti-cracking steel structure fire retardant coating is brushed on the surface of the substrate, and after brushing, it is cured for 1 to 5 days, and then baked at 60 to 120° C. for 1 to 3 days to obtain a high temperature resistant intumescent, enhanced anti-cracking steel structure fire retardant coating.

[0058] Furthermore, the substrate includes buildings, vehicles, panels and various objects that require fire protection.

[0059] The present invention has the following beneficial effects:

[0060] (1) The method of grafting modified chopped fibers with phosphorylated POSS-based flame retardants in the present invention is stable and reliable, imparting flame retardant properties to chopped carbon fibers, effectively improving their dispersibility in matrix materials and compatibility with matrix materials, and the well-dispersed flame-retardant modified chopped fibers are expected to solve the problem of easy cracking of fire-retardant coatings on steel structures;

[0061] (2) In the present invention, the UiO-66 hybrid nanomaterial is modified with an intumescent flame retardant to effectively enhance the flame retardant properties of the UiO-66 nanomaterial, and is organically combined with the metal-catalyzed carbonization, smoke suppression and toxicity reduction, and adsorption properties of the metal organic framework itself, thereby improving the flame retardant properties of the intumescent fire retardant coating in a diversified manner;

[0062] (3) In the present invention, the intumescent steel structure fire retardant coating containing phosphorylated POSS-based flame retardant grafted modified chopped fibers and intumescent flame retardant modified UiO-66 hybrid nanomaterials exerts a synergistic and efficient flame retardant effect, thereby comprehensively improving the fire safety performance of the steel structure fire retardant coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 Infrared spectra of UiO-66 before and after modification.

[0064] Figure 2 XRD patterns of UiO-66 before and after modification.

[0065] Figure 3 These are SEM images of UiO-66 before and after modification, where a is before flame retardant modification and b is after flame retardant modification.

[0066] Figure 4 These are SEM images of carbon fiber before and after modification, where a is 200um carbon fiber before flame retardant modification, and b is 200um carbon fiber after flame retardant modification.

[0067] Figure 5 These are photos of the modified resin before and after the cone calorimetry test, where a is the pure epoxy resin sample and b is the epoxy resin modified with nanomaterials. DETAILED DESCRIPTION

[0068] The present invention is further explained and illustrated below in conjunction with the attached tables and examples, but the protection scope of the present invention is not limited to the following examples.

[0069] Example 1

[0070] A method for preparing phosphorylated POSS-based flame retardant grafted modified short fibers comprises the following steps:

[0071] 1. Synthesis of A-POSS solid.

[0072] 90 mL of 3-aminopropyltriethoxysilane (APTES) was completely dissolved in 700 mL of anhydrous methanol solution, mixed with 123 mL of hydrochloric acid solution and stirred for 3 days, and allowed to react for 10 days. After solid-liquid separation, the obtained product was A-POSS solid.

[0073] 2. Preparation of phosphorylated POSS-based flame retardant grafted modified chopped fibers.

[0074] 3.52g A-POSS solid was completely dissolved in 500mL deionized water, the temperature was raised to 45°C, 26g formaldehyde solution was added, and the mixture was stirred for 30min. The temperature was then raised to 55°C, 5.853g phosphorous acid was added, and after the solution was clarified, 0.2mm chopped carbon fiber was added. The temperature was raised to 85°C, and the mixture was stirred for 12h. After solid-liquid separation and drying, the obtained fiber material was the flame-retardant modified chopped carbon fiber material.

[0075] A method for preparing a UiO-66 hybrid nanomaterial loaded with an intumescent flame retardant coating comprises the following steps:

[0076] 1. Preparation of UiO-66 micro-nano materials.

[0077] 0.714 g zirconium chloride and 0.5075 g 2-aminoterephthalic acid were dissolved in 80 mL of N,N-dimethylformamide solution respectively and mixed evenly, and reacted at 120°C for 12 hours to obtain a clear suspension; the suspension was centrifuged at a speed of 3000 r / min for 6 minutes to collect the precipitate, and washed 3 times with methanol solution, and finally the obtained solid was dried in a vacuum oven at 80°C for 2 hours. The obtained product is the UiO-66 metal organic framework material.

[0078] 2. Preparation of flame retardant modified solution.

[0079] 1 g of chitosan powder was weighed and dissolved in 100 mL of 1 wt % acetic acid solution to prepare a chitosan solution with a concentration of 1 wt %; 2 g of ammonium polyphosphate was weighed and dissolved in 100 mL of deionized water to prepare an ammonium polyphosphate solution with a concentration of 2 wt %.

[0080] 3. Preparation of UiO-66 hybrid nanomaterials loaded with intumescent flame retardant coating.

[0081] (1) The obtained UiO-66 sample was immersed in the prepared 1 wt% chitosan solution for 5 min, and the particle precipitate was collected and washed with deionized water to remove the unadsorbed chitosan particles;

[0082] (2) The precipitate obtained in (1) was immersed in a prepared 2 wt% ammonium polyphosphate solution for 5 min, and then the particle precipitate was collected and washed with deionized water to remove the unabsorbed ammonium polyphosphate particles, thereby completing the expansion flame retardant modification of the UiO-66 nanomaterial;

[0083] (3) Repeat the assembly process of steps (1) to (2), shortening the immersion time to 1 min, until 5 modifications are achieved.

[0084] A method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66 comprises the following steps:

[0085] Weigh 47.383g of epoxy resin, 2.0g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped carbon fiber, and 10.617g of 4,4-diaminodiphenylmethane, stir and mix until uniform, mechanically stir and disperse for 5h to form a uniformly dispersed intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped carbon fiber and modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped carbon fiber and modified UiO-66.

[0086] Example 2

[0087] A method for preparing phosphorylated POSS-based flame retardant grafted modified short fibers, prepared by referring to the steps in Example 1;

[0088] A method for preparing a UiO-66 hybrid nanomaterial loaded with an intumescent flame retardant coating, prepared by referring to the steps in Example 1;

[0089] A method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66 comprises the following steps:

[0090] Weigh 47.791g of epoxy resin, 1.2g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped carbon fiber, and 10.709g of 4,4-diaminodiphenylmethane, stir and mix until uniform, mechanically stir and disperse for 5h to form a uniformly dispersed intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66.

[0091] Example 3

[0092] A method for preparing phosphorylated POSS-based flame retardant grafted modified short fibers, prepared by referring to the steps in Example 1;

[0093] A method for preparing a UiO-66 hybrid nanomaterial loaded with an intumescent flame retardant coating, prepared by referring to the steps in Example 1;

[0094] A method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66 comprises the following steps:

[0095] Weigh 48.284g of epoxy resin, 0.6g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped carbon fiber, and 10.516g of 4,4-diaminodiphenylmethane, stir and mix until uniform, mechanically stir and disperse for 5h to form a uniformly dispersed intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66.

[0096] Example 4

[0097] A method for preparing phosphorylated POSS-based flame retardant grafted modified short fibers, prepared by referring to the steps in Example 1;

[0098] A method for preparing a UiO-66 hybrid nanomaterial loaded with an intumescent flame retardant coating, prepared by referring to the steps in Example 1;

[0099] A method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66 comprises the following steps:

[0100] Weigh 48.530g of epoxy resin, 0.3g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped carbon fiber, and 10.570g of 4,4-diaminodiphenylmethane, stir and mix until uniform, mechanically stir and disperse for 5h to form a uniformly dispersed intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120°C for 1 day to obtain a high temperature resistant intumescent and reinforced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66.

[0101] Comparative Example 1

[0102] Weigh 49.269g of epoxy resin and 10.731g of 4,4-diaminodiphenylmethane and stir and mix them until uniform, and mechanically stir to form a uniformly dispersed resin coating. Apply the uniformly mixed resin coating to the pretreated substrate surface by brushing. After brushing, cure at room temperature for 3 days and bake at 120°C for 1 day to obtain a coating.

[0103] Comparative Example 2

[0104] Weigh 48.777g of epoxy resin, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped carbon fiber, and 10.623g of 4,4-diaminodiphenylmethane, stir and mix until uniform, and mechanically stir and disperse for 5h to form a uniformly dispersed reinforced anti-cracking steel structure fire retardant coating with added flame-retardant chopped carbon fiber. Apply the uniformly mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120°C for 1 day to obtain a reinforced anti-cracking steel structure fire retardant coating with added flame-retardant chopped fibers.

[0105] Comparative Example 3

[0106] Weigh 48.284g of epoxy resin, 1.2g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating and 10.516g of 4,4-diaminodiphenylmethane and stir and mix until uniform, mechanically stir and disperse for 5h to form an intumescent, enhanced anti-cracking steel structure fire retardant coating of modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent steel structure fire retardant coating of modified UiO-66.

[0107] Comparative Example 4

[0108] Weigh 48.284g of epoxy resin, 1.2g of UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, 0.6g of 0.2mm chopped carbon fiber, and 10.516g of 4,4-diaminodiphenylmethane, stir and mix until uniform, and mechanically stir and disperse for 5h to form a uniformly dispersed intumescent and enhanced anti-cracking steel structure fire retardant coating with added chopped carbon fiber and modified UiO-66. Apply the mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent and enhanced anti-cracking steel structure fire retardant coating with added chopped carbon fiber and modified UiO-66.

[0109] Comparative Example 5

[0110] Weigh 48.284g of epoxy resin, 1.2g of UiO-66 nanomaterial, 0.6g of 0.2mm phosphorylated POSS-based flame retardant grafted modified chopped fibers, and 10.570g of 4,4-diaminodiphenylmethane, stir and mix until uniform, and mechanically stir and disperse for 5h to form a uniformly dispersed enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and UiO-66. The mixed fire retardant coating is brushed on the surface of the pretreated substrate, and after brushing, it is cured at room temperature for 3 days and baked at 120°C for 1 day to obtain a high temperature resistant enhanced anti-cracking steel structure fire retardant coating with added flame retardant chopped fibers and modified UiO-66.

[0111] Comparative Example 6

[0112] Weigh 48.284g of epoxy resin, 1.2g of ammonium polyphosphate / chitosan intumescent flame retardant mixed material, and 10.570g of 4,4-diaminodiphenylmethane, stir and mix until uniform, and mechanically stir and disperse for 5h to form a uniformly dispersed intumescent steel structure fire retardant coating. Apply the uniformly mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant intumescent steel structure fire retardant coating.

[0113] Comparative Example 7

[0114] Weigh 48.284g of epoxy resin, 1.2g of ammonium polyphosphate / pentaerythritol traditional intumescent flame retardant mixed material, and 10.570g of 4,4-diaminodiphenylmethane, stir and mix until uniform, and mechanically stir and disperse for 5h to form a uniformly dispersed traditional intumescent steel structure fire retardant coating. Apply the uniformly mixed fire retardant coating to the pretreated substrate surface, cure at room temperature for 3 days after brushing, and bake at 120℃ for 1 day to obtain a high temperature resistant traditional intumescent steel structure fire retardant coating.

[0115] Table 1 Comparative Examples 1 to 7 and Examples 1 to 3 Sample Formulas

[0116]

[0117]

[0118] Results

[0119] Cone calorimetry test detection process: The composite material samples prepared in Examples 1 to 4 and Comparative Examples 1 to 7 were respectively installed on the test device, the power of the radiation cone was set to 35 kW, the cone calorimeter was started, thermal radiation was performed and test data was collected in real time, and parameters such as the heat release rate (PHRR), total heat release (THR), total smoke release (TSR) and real-time mass (MASS) of the material were calculated. After the preset test time was reached, the thermal radiation of the radiation cone was stopped, and the following data were obtained:

[0120] Table 2 Cone calorimetry test data of comparative examples 1 to 7 and examples 1 to 3

[0121]

[0122] The peak heat release rate (PHRR) indicates the typical combustion characteristics of the material. Compared with the comparative pure epoxy resin (Comparative Example 1), the PHRR value of the embodiment is high, which proves that after adding the expanded flame retardant modified UiO-66 nano flame retardant system and the flame retardant modified short fibers, the flame retardant properties are improved, and the flame retardant properties of the composite material with the flame retardant modified short fibers added alone are also improved; the PHRR values ​​of Examples 2 to 4 gradually improve with the increase of the amount of expanded flame retardant modified UiO-66 added, which proves that within a certain range, the flame retardant properties are enhanced with the increase of the amount of expanded flame retardant modified UiO-66 nano flame retardant system added, however, when the amount of expanded flame retardant modified UiO-66 added is further increased ( In Example 1), the flame retardant performance deteriorates, which may be caused by the agglomeration phenomenon caused by excessive addition of nanoparticles; compared with Comparative Examples 3 to 4, Example 2 adds the same amount of intumescent flame retardant modified UiO-66, and the flame retardant modified short fibers are better than adding no addition and adding ordinary short fibers; compared with Comparative Example 2, Example 3 and Comparative Examples 5 to 7 add the same amount of flame retardant modified short fibers. The effect of adding UiO-66 nano flame retardant modified by intumescent flame retardant is better than that of the composite material with nanomaterials added alone, the intumescent flame retardant (APP / CS) used for modification, and the traditional intumescent flame retardant (APP / pentaerythritol). The intumescent effect of the composite material with UiO-66 nano flame retardant modified by intumescent flame retardant is as follows: Figure 5 As shown in (b), the UiO-66 nano flame retardant is an integrated expansion flame retardant system, which synergistically plays the role of dehydrating agent / foaming agent to form a stable expansion carbon layer to protect the base material from continuous impact of flame and heat. In summary, the composite material of the UiO-66 metal frame modified by a certain amount of APP / CS expansion flame retardant and the flame retardant modified short fiber shows excellent flame retardant properties, while the flame retardant properties of the UiO-66 metal frame modified by APP / CS expansion flame retardant and the flame retardant modified short fiber alone, as well as the composite material added with general expansion flame retardant, nanomaterials and carbon fiber effect are not good enough.

[0123] Similarly, the above conclusion can also be drawn through values ​​such as the total heat release (THR) that represents the total amount of heat released from the ignition of the material to the extinction of the flame, and the real-time mass (mass) that represents the trend of decomposition and weight loss during the combustion process of the material.

[0124] Strength test detection process: respectively take the fireproof composite material samples prepared in Examples 1 to 3 and Comparative Examples 1 to 7, clamp and fix them on the test device, apply tension, gradually increase the load until the sample breaks, record the changes in load and displacement during the test, and obtain the following data:

[0125] Table 3 Strength test data of comparative examples and embodiments 1 to 3

[0126]

[0127] The introduction of a certain amount of nanomaterials and reinforced chopped fibers into composite materials can effectively enhance the mechanical properties of composite materials. As shown in the above table, the tensile strength, tensile modulus and elongation at break of all samples with chopped fibers added, whether modified or not (except Example 1), have increased. When the amount of chopped fibers added is constant, the strength of Examples 2 to 4 increases with the increase in the amount of expanded flame-retardant modified UiO-66 added. This is because the introduction of nanomaterials can increase the interface effect and thus improve the mechanical properties. However, in Example 1, when the amount of expanded flame-retardant modified UiO-66 added exceeds a certain range, a large amount of nanomaterials agglomerate and cause stress concentration, thereby causing the mechanical properties of the composite material to deteriorate; For Comparative Examples 2 to 7, since no chopped fibers are added in Comparative Example 3 but nanomaterials are added, the mechanical properties are slightly improved compared to Comparative Example 1, and the data of Comparative Examples 4 to 5 are better than those of Comparative Examples 2 and Comparative Examples 6 to 7, indicating that nanomaterials are beneficial to enhancing the mechanical properties of composite materials.

[0128] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing an intumescent, enhanced anti-cracking steel structure fire retardant coating, characterized in that: The steps include: Ⅰ. Preparation of base material: weigh the film former and curing agent and stir until a uniformly mixed base material is obtained; II. Preparation of intumescent, enhanced anti-cracking steel structure fire retardant coating: Take the base material and the UiO-66 hybrid nanomaterial loaded with intumescent flame retardant coating, mix and stir to form a uniform dispersion system; then, add the flame retardant modified chopped carbon fiber material to the uniform dispersion system and disperse it evenly to obtain the intumescent, enhanced anti-cracking steel structure fire retardant coating; The flame retardant modified chopped carbon fiber material accounts for 0.5-10% of the uniformly dispersed system; The UiO-66 hybrid nanomaterial loaded with the intumescent flame retardant coating accounts for 1 to 8.0% of the total weight of the uniformly dispersed system; The method for preparing the flame retardant modified chopped carbon fiber material comprises the following steps: 1) Synthesis of A-POSS solid: 3-aminopropyltriethoxysilane is dissolved in anhydrous methanol solution, mixed with hydrochloric acid solution, allowed to react for a period of time, and after solid-liquid separation, the obtained product is A-POSS solid; 2) Preparation of phosphorylated POSS-based flame retardant grafted modified chopped fibers: dissolve the A-POSS solid obtained in step 1 in water, heat to 45-50° C., add formaldehyde, stir thoroughly for 30-40 min, then heat to 55-60° C., add phosphorous acid, after the solution is clarified, add chopped carbon fibers, heat to 85-95° C., stir to react, separate the solid from the liquid and dry, and the obtained fiber material is a flame retardant modified chopped carbon fiber material; The method for preparing the UiO-66 hybrid nanomaterial loaded with an expansion flame retardant coating comprises the following steps: S1. Preparation of UiO-66 micro-nano material: dissolving the transition metal salt compound and the organic ligand in a solvent respectively and mixing them evenly, reacting them under a certain temperature condition to obtain a suspension; collecting the suspension by centrifugation to precipitate, washing it with methanol or water for multiple times, and finally drying the obtained solid to obtain the product, which is the UiO-66 micro-nano material; S2. Preparation of flame retardant modified solution: dissolving chitosan in a solvent to prepare a chitosan solution of a certain concentration; dissolving ammonium polyphosphate in a solvent to prepare an ammonium polyphosphate solution of a certain concentration; S3. Preparation of UiO-66 hybrid nanomaterials loaded with intumescent flame retardant coating: a. Immersing the UiO-66 micro-nano material obtained in step S1 in the chitosan solution in step S2, and then collecting and washing the particle precipitate to remove the unadsorbed chitosan particles; b. Immersing the particle precipitate obtained in step a in the prepared ammonium polyphosphate solution, collecting the particle precipitate after a certain period of time and washing it to remove the unabsorbed ammonium polyphosphate particles, thus completing the expansion flame retardant modification of the UiO-66 nanomaterial; c. Repeat steps a to b 3 to 10 times.

2. The preparation method according to claim 1, characterized in that: In step I, the film-forming agent includes one or more of epoxy resin, polyurethane, acrylic acid, and water-based silicone acrylic emulsion; the curing agent includes one or more of ethylenediamine, diethylenetriamine, triethylenetetramine, and 4,4-diaminodiphenylmethane; the ratio of the film-forming agent to the curing agent is 1.5:1 to 5:

1.

3. The preparation method according to claim 1, characterized in that: In step 1, the volume ratio of 3-aminopropyltriethoxysilane to anhydrous methanol is 1:7.8 to 1:10; the ratio of 3-aminopropyltriethoxysilane to hydrochloric acid solution is 1:1.4 to 1:

2.

4. The preparation method according to claim 1, characterized in that: In step 2, the mass ratio of the A-POSS solid to water is 1:100 to 20:100; the molar ratio of the NH bonds in the A-POSS solid to formaldehyde is 1:16 to 1:32; and the molar ratio of the NH bonds in the A-POSS solid to phosphorous acid is 1:16 to 1:

32.

5. The preparation method according to claim 1, characterized in that: In step 2, the length of the chopped carbon fiber is 0.1 to 10 mm.

6. The preparation method according to claim 1, characterized in that: In step S1, the transition metal salt compound is one or more of metal zirconium salts such as zirconium chloride, zirconium sulfate, zirconium acetate, etc.; the organic ligand is one or more of terephthalic acid, trimesic acid and dimethylimidazole; the solvent is one or more of water, methanol, anhydrous ethanol and N,N-dimethylformamide.

7. The preparation method according to claim 1, characterized in that: In step S1, the concentration of the transition metal salt compound in the suspension is 0.01-0.05 mol / L; the concentration of the organic ligand in the suspension is 0.01-0.05 mol / L.

8. The preparation method according to claim 1, characterized in that: In step S2, the solvent is one or more of water, acetic acid, and N,N-dimethylformamide; the concentration of the chitosan solution is 0.5-5wt%; and the concentration of the ammonium polyphosphate solution is 0.5-5wt%.

9. An intumescent, enhanced anti-cracking steel structure fire retardant coating, characterized in that: The intumescent, enhanced anti-cracking steel structure fire retardant coating is prepared according to the preparation method described in any one of claims 1 to 8.

10. Use of the intumescent, enhanced anti-cracking steel structure fire retardant coating as claimed in claim 9 in the field of fire prevention and fire retardant product preparation.

Citation Information

Patent Citations

  • Low-creep flame-retardant damping rubber and preparation method thereof

    CN111621068A

  • Flame retardant and preparation method thereof, and flame-retardant epoxy resin and preparation method thereof

    CN112592492A

  • Preparation method of high-temperature-resistant CNPU-TEOS water-based intumescent fireproof coating

    CN116333559A

  • METHOD FOR PREPARING COATED MOFs BY SELF-ASSEMBLY OF INTUMESCENT FLAME RETARDANT

    US20230174866A1