Anti-bleeding sand-in-water coating and preparation method thereof
Through the reaction of hydrophobic modified cellulose, hydroxyethyl cellulose and S482 protective glue and the combination of sodium tetraborate decahydrate and modified guar gum, a stable gel layer and a three-dimensional network structure are formed, solving the problem of water-in-sand coating The problem of poor toughness of medium-colored particles is achieved, and good anti-bleeding performance and adhesion are achieved.
Patent Information
- Application Number
- CN202410773832.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-17
AI Technical Summary
The colored particles in existing water-in-sand coatings have poor toughness, which results in the occurrence of broken particles during the granulation process, which in turn causes the coating to bleed.
Hydrophobic modified cellulose, hydroxyethyl cellulose and S482 protective glue are used to react with each other to form a gel mass, which is wrapped around the calcined colored sand. The thickness of the gel layer is increased through the reaction between acrylic emulsion and S482 protective glue, combined with tetraboric acid decahydrate. Sodium and modified guar gum form a stable three-dimensional network structure to improve the toughness and adhesion of color particles.
It effectively prevents the calcined colored sand from breaking during the granulation process, improves the anti-bleeding performance and adhesion of water-in-sand coatings, and enhances the strength and wash resistance of the paint film.
Smart Images

Figure BDA0004894938040000091 
Figure BDA0004894938040000101
Abstract
Description
Technical Field
[0001] The invention relates to the field of exterior wall decorative coatings, in particular to an anti-color seepage water-coated sand coating and a preparation method thereof. Background Art
[0002] Water-based sand paint is a kind of paint composed of water-based emulsion, sand and additives. Its appearance and texture are similar to real stone paint, but the sand particles of water-based sand are smaller and the paint surface is more delicate. Therefore, water-based sand paint is suitable for indoor and outdoor wall, column, line and other decorations, especially suitable for construction on flat or slightly flat surfaces.
[0003] Existing water-based sand multi-color paints mostly use color paste to wrap white sand as color particles. There are problems when using color paste to adjust colors: there is a lot of wetting agent in the color paste. When darkening color particles, a large amount of color paste is added, resulting in more wetting agent being brought in. The increase in wetting agent will reduce the gelation of the color particles and reduce the toughness of the color particles. The color particles are prone to breakage during the granulation process, which will cause the paint to bleed. Summary of the invention
[0004] In order to solve the problem of poor toughness of color particles in existing water-in-sand coatings, the present invention provides an anti-color seepage water-in-sand coating and a preparation method thereof.
[0005] The present invention provides an anti-color seepage water-coated sand coating and a preparation method thereof, which adopts the following technical solutions: An anti-bleeding water-in-sand paint comprises the following raw materials in parts by weight: 550-650 parts of a base paint, 200-300 parts of a granulating liquid, and 100-200 parts of a continuous phase, wherein the base paint comprises 296-336 parts of water, 2-5 parts of a fungicide, 1-3 parts of a dispersant, 5-8 parts of titanium dioxide, 3-5 parts of a defoamer, 3-5 parts of hydrophobically modified cellulose, 4-5 parts of hydroxyethyl cellulose, 10-14 parts of ethylene glycol, 10-15 parts of a film-forming aid, 1-2 parts of a multifunctional aid, 160-200 parts of an acrylic emulsion, 3-5 parts of an S482 protective glue, 0.1-0.2 parts of a wetting agent, 420-460 parts of 80-120 mesh calcined colored sand, 1-3 parts of modified guar gum, and 1-3 parts of sodium tetraborate decahydrate; The bactericide consists of a DMB long-acting bactericide and a HF fast bactericide.
[0006] By adopting the above technical scheme, hydrophobically modified cellulose, hydroxyethyl cellulose and S482 protective glue react with each other, and the negative charge on the surface of S482 protective glue forms a dipole interaction with the hydroxyl polar group to form a gel group with a certain strength and insoluble in water. The mesh structure between the gel groups wraps the calcined colored sand, so that a gel layer is formed on the outer surface of the calcined colored sand. The reaction of acrylic emulsion and S482 protective glue can increase the thickness of the gel layer, which has a better protective effect on the calcined colored sand, thereby preventing the calcined colored sand from breaking into particles during the granulation process, and making the water-based sand coating have good anti-color penetration performance. In addition, sodium tetraborate decahydrate combines with the hydroxyl groups on the modified guar gum molecular chain to form an interwoven stable three-dimensional spatial mesh structure, which can effectively improve the adhesion of the water-based sand coating, and at the same time can also strengthen the mesh structure between the gel groups, effectively improving the toughness of the color particles.
[0007] Preferably, the modified guar gum is obtained by the following preparation method: S1: dissolving 35-45 g of tetraethylene glycol in 50 ml of tetrahydrofuran, dissolving 8-12 g of sodium hydroxide in 60 ml of water to form an aqueous sodium hydroxide solution, mixing the tetrahydrofuran solution containing tetraethylene glycol and the aqueous sodium hydroxide solution under ice bath conditions, then adding tetrahydrofuran dissolved with toluene-4-sulfonyl chloride dropwise, keeping the ice bath stirring for 3-4 hours, extracting the reaction solution obtained by the reaction with dichloromethane, then removing water, and filtering to obtain an activated tetraethylene glycol solution; S2: 2-3 g of guar gum is added to 3-4 g of isopropanol and stirred. After adding 0.3-0.5 g of sodium hydroxide at a temperature of 25-30° C. for alkalization for 20-30 minutes, the activated tetraethylene glycol solution obtained in step S1 is added under a temperature of 50-55° C. and reacted for 3-5 hours. The modified guar gum is filtered and dried.
[0008] Guar gum has a slow dissolution rate due to the hydrogen bonding within the molecule, and spherical micelles and bubbles appear during dissolution. After the guar gum is modified by the above technical solution, the hydrophilicity of the guar gum is increased, and the modification process improves the hydrogen bonding within the guar gum molecule, so that the dissolution rate of the modified guar gum is improved. After the modified guar gum is completely swollen, the molecular action and entanglement increase the intermolecular force, thereby making the water-based sand coating more stable. In addition, the three-dimensional spatial network structure formed by the reaction of the modified guar gum and sodium tetraborate decahydrate has an improved shear resistance, which can further prevent the colored sand particles from breaking during the granulation process.
[0009] Preferably, the calcined colored sand is obtained by the following preparation method: S1: adding 3-5 parts by weight of a pigment to 15-25 parts by weight of an aqueous solution containing 10-20 wt% of an aqueous hyperdispersant, and obtaining a pigment paste by ultrasonic dispersion; S2: Add 8-10 parts by weight of aluminum dihydrogen phosphate and 0.3-0.5 parts by weight of boric acid into 100 parts by weight of quartz sand, then add the pigment paste obtained in step S1, stir evenly, and calcine at 600-700° C. for 3-5 hours to obtain calcined colored sand.
[0010] By adopting the above technical solution, after the pigment is dispersed through the aqueous dispersant, the pigment is more completely coated on the surface of the natural sand and can be more evenly attached to the surface of the natural sand. The addition of aluminum dihydrogen phosphate can increase the bonding strength between the quartz sand and the pigment paste, reduce the probability of pigment shedding, and improve the wear resistance of the calcined colored sand.
[0011] Preferably, the hydrophobically modified cellulose comprises HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose in a weight ratio of 1:2.
[0012] By adopting the above technical solution, the hydrophobically modified cellulose is composed of HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose, which can effectively improve the wrapping effect on the calcined colored sand and reduce color penetration.
[0013] Preferably, the granulation liquid comprises, by weight, 1000 parts of water, 1-2 parts of long-acting fungicide, 20-30 parts of S80 protective glue, 1-2 parts of xanthan gum, 1-1.5 parts of carboxymethyl cellulose, 1-2 parts of multifunctional auxiliary agent, and 1-2 parts of rapid fungicide.
[0014] Preferably, the continuous phase includes, by weight, 240-260 parts of water, 1-2 parts of long-acting bactericide, 25-35 parts of nanocellulose, 1-2 parts of Plus330 hydrophobically modified cellulose, 25-35 parts of ethylene glycol, 25-35 parts of film-forming aid, 1-2 parts of multifunctional aid, 430-460 parts of RS-3799A emulsion, 180-220 parts of RS-3765 emulsion, 2-4 parts of fast bactericide, 2-3 parts of thickener, and 10-30 parts of silica sol.
[0015] By adopting the above technical solution, after adding silica sol to the continuous phase, the combination of silica sol, cellulose and emulsion can form a more stable hardened protective layer on the surface of the color particles with high density, thereby effectively improving the strength of the water-based sand coating.
[0016] The second aspect of the present invention is to provide a method for preparing an anti-color seepage water-in-sand coating, comprising the following steps: S1: Prepare the base paint S11: Mix S482 protective glue with part of water, and disperse for 40-50 minutes at a rotation speed of 1200±10r / min to form a protective glue solution with a concentration of 10%; S12: Stir and mix the remaining water, long-acting fungicide, dispersant and defoamer at a speed of 300±10r / min, then add titanium dioxide, hydrophobically modified cellulose and hydroxyethyl cellulose while stirring, then adjust the speed to 500±10r / min, continue stirring for 5-10min, then add ethylene glycol, film-forming aid and multifunctional aid, then adjust the speed to 1300r / min and disperse for 5-15 minutes; S13: Add acrylic emulsion to the solution obtained in step S12, lower the speed to 800±10r / min, and stir for 5-10min; S14: squeeze the protective glue solution, modified guar gum and sodium tetraborate decahydrate obtained in step S11 into the solution obtained in step S13, and then adjust the speed to 1200±10r / min for dispersion for 5-10min; S15: adding a rapid bactericide, a wetting agent and calcined colored sand to the solution obtained in step S14 to obtain a base paint; S2: mixing the base paint and the granulation liquid to obtain color particles; S3: Add the continuous phase to step S2, and stir and mix to obtain the water-in-sand coating.
[0017] Preferably, the granulation liquid is prepared as follows: by weight, 500 parts of water and 1-2 parts of long-acting fungicide are stirred and mixed uniformly, 20-30 parts of S80 protective glue, 1-2 parts of xanthan gum, and 1-1.5 parts of carboxymethyl cellulose are added at a speed of 800±10r / min, and after dispersion for 5-10 minutes, 1-2 parts of multifunctional auxiliary agent are added, the speed is adjusted to 1300r / min, and after dispersion for 35-45min, 1-2 parts of rapid fungicide and 500 parts of water are added, the speed is adjusted to 400r / min, and the dispersion is carried out for 5min to obtain the granulation liquid.
[0018] Preferably, the continuous phase is prepared as follows: by weight, 240-260 parts of water and 1-2 parts of long-acting fungicide are mixed at a speed of 500r / min, and then 25-35 parts of nanocellulose and 1-2 parts of hydrophobically modified cellulose are added and stirred for 5-10min, and then 25-25 parts of ethylene glycol, 25-35 parts of film-forming aids, and 1-2 parts of multifunctional aids are added, and the speed is adjusted to 1300r / min and stirred and dispersed for 10-20min, and then the speed is adjusted to 600r / min, and then 430-460 parts of RS-3799A emulsion, 180-220 parts of RS-3765 emulsion, 2-4 parts of fast fungicide, 2-3 parts of thickener, and 10-30 parts of silica sol are added, and the continuous phase is obtained after stirring and mixing for 5-10 minutes.
[0019] In summary, the present invention has the following beneficial effects: the addition of modified guar gum and sodium tetraborate decahydrate in the base paint of the present application can strengthen the gel layer formed by the reaction of S482 protective glue with cellulose and emulsion, improve the toughness of the color particles, thereby reducing the occurrence of broken particles in the calcined colored sand during the granulation process, thereby effectively ensuring the anti-color penetration performance of the water-based sand coating, and the addition of silica sol in the continuous phase can make the silica sol, cellulose and emulsion used in combination, and can form a more stable hardened protective layer on the surface of the color particles with high density, thereby effectively improving the strength and adhesion of the water-based sand coating. DETAILED DESCRIPTION
[0020] The present invention is further described in detail below with reference to the embodiments.
[0021] The raw materials used in the preparation examples, embodiments and comparative examples of this application are all commercially available.
[0022] The dispersant was purchased from BASF, model N40; The multifunctional additive was purchased from Solvay, model MP380; The long-acting fungicide was purchased from Oshada Chemical, model number DMB; HE-10K hydrophobically modified cellulose was purchased from Ashland; HM-10K hydrophobically modified cellulose was purchased from Shandong Yunying; Acrylic emulsion was purchased from Showa, Japan, model number AP-4765; 80-120 mesh calcined colored sand was purchased from Guangdong Shuangjiang; RS-3799A emulsion and RS-3765 emulsion were purchased from Badfu; The thickener was purchased from Dow Chemical, model number TT935; The film-forming aid was purchased from Runtai Chemical; The defoamer was purchased from Deqian, model number AP7010; S482 protective glue and S80 protective glue were purchased from Jiangsu Hemmings; Carboxymethyl cellulose was purchased from Akzo Nobel, model 4000G; Modified guar gum was purchased from Wuhan Penglei Biotechnology Co., Ltd.; Silica sol was purchased from Orun Chemical, model number S308.
[0023] Preparation Example 1 The preparation method of modified guar gum comprises the following preparation steps: S1: 35 g of tetraethylene glycol is dissolved in 50 ml of tetrahydrofuran, 8 g of sodium hydroxide is dissolved in 60 ml of water to form a sodium hydroxide aqueous solution, the tetrahydrofuran solution containing tetraethylene glycol and the sodium hydroxide aqueous solution are mixed under ice bath conditions, and then tetrahydrofuran dissolved with toluene-4-sulfonyl chloride is added dropwise, and the reaction is stirred in an ice bath for 3 hours, and the reaction solution obtained by the reaction is extracted with dichloromethane, and then water is removed and suction filtered to obtain an activated tetraethylene glycol solution; S2: 2 g of guar gum was added to 3 g of isopropanol and stirred. After alkalization for 20 minutes at 25° C., 0.3 g of sodium hydroxide was added. After the temperature was raised to 50° C., the activated tetraethylene glycol solution obtained in step S1 was added and reacted for 3 hours. The modified guar gum was filtered and dried.
[0024] Preparation Example 2 The preparation method of modified guar gum comprises the following preparation steps: S1: 45 g of tetraethylene glycol is dissolved in 50 ml of tetrahydrofuran, 12 g of sodium hydroxide is dissolved in 60 ml of water to form a sodium hydroxide aqueous solution, the tetrahydrofuran solution containing tetraethylene glycol and the sodium hydroxide aqueous solution are mixed under ice bath conditions, and then tetrahydrofuran dissolved with toluene-4-sulfonyl chloride is added dropwise, the reaction is stirred in an ice bath for 4 hours, the reaction solution obtained by the reaction is extracted with dichloromethane, and then water is removed and suction filtered to obtain an activated tetraethylene glycol solution; S2: 3 g of guar gum was added to 4 g of isopropanol and stirred. After alkalization for 30 minutes, 0.5 g of sodium hydroxide was added at 30° C., and then the activated tetraethylene glycol solution obtained in step S1 was added under the condition of heating to 55° C. to react for 5 hours. The modified guar gum was obtained by suction filtration and drying.
[0025] Preparation Example 3 The preparation method of calcined colored sand comprises the following preparation steps: S1: 3 kg of pigment is added to 15 kg of aqueous solution containing 10 wt% of aqueous hyperdispersant, and the pigment paste is obtained by ultrasonic dispersion; the physical properties of the aqueous hyperdispersant are: viscosity 98 mPa·s, Ph8.3, active ingredient content 46±2%, density 1.13 kg / m 3 ; S2: Add 8 kg of aluminum dihydrogen phosphate and 0.3 kg of boric acid into 100 kg of quartz sand, then add the pigment paste obtained in step S1, stir evenly, and calcine at 600° C. for 3 h to obtain calcined colored sand.
[0026] Preparation Example 4 The preparation method of calcined colored sand comprises the following preparation steps: S1: 5 kg of pigment is added to 25 kg of aqueous solution containing 20 wt% of aqueous hyperdispersant, and the pigment paste is obtained by ultrasonic dispersion; the physical properties of the aqueous hyperdispersant are: viscosity 98 mPa·s, Ph8.3, active ingredient content 46±2%, density 1.13 kg / m 3 ; S2: Add 10 kg of aluminum dihydrogen phosphate and 0.5 kg of boric acid into 100 kg of quartz sand, then add the pigment paste obtained in step S1, stir evenly, and calcine at 700° C. for 5 hours to obtain calcined colored sand.
[0027] Example 1 A method for preparing an anti-color seepage water-in-sand coating comprises the following steps: S1: Prepare the base paint S11: 3 kg of S482 protective glue was mixed with 27 kg of water, and dispersed at a speed of 1200 ± 10 r / min for 40 minutes to form a protective glue solution with a concentration of 10%; S12: 269 kg of water, 0.7 kg of long-acting fungicide, 1 kg of dispersant, and 1.5 kg of defoamer are stirred and mixed at a speed of 300 ± 10 r / min, and then 5 kg of titanium dioxide, 3 kg of hydrophobically modified cellulose, and 4 kg of hydroxyethyl cellulose are added while stirring, and then the speed is adjusted to 500 ± 10 r / min, and stirring is continued for 5 minutes, and then 10 kg of ethylene glycol, 10 kg of film-forming aid, and 1 kg of multifunctional aid are added, and then the speed is adjusted to 1300 r / min and dispersed for 5 minutes; wherein the hydrophobically modified cellulose is composed of HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose in a weight ratio of 1:2; S13: Add 160 kg of acrylic emulsion to the solution obtained in step S12, reduce the rotation speed to 800 ± 10 r / min, and stir for 5 min; S14: squeeze the protective glue solution obtained in step S11, 1 kg of modified guar gum, and 1 kg of sodium tetraborate decahydrate into the solution obtained in step S13, and then adjust the speed to 1200±10 r / min and disperse for 5 minutes; S15: Add 1.5 kg of defoamer, 1.3 kg of rapid bactericide, 0.1 kg of wetting agent and 420 kg of 80-120 mesh calcined colored sand to the solution obtained in step S14 to obtain a base paint; S2: Preparation of granulation liquid: 500 kg of water and 1 kg of long-acting fungicide were stirred and mixed evenly, 20 kg of S80 protective glue, 1 kg of xanthan gum and 1 kg of carboxymethyl cellulose were added at a speed of 800 ± 10 r / min, and after dispersion for 5 minutes, 1 kg of multifunctional auxiliary agent was added, the speed was adjusted to 1300 r / min, and after dispersion for 35 minutes, 1 kg of rapid fungicide and 500 kg of water were added, the speed was adjusted to 400 r / min, and dispersion was carried out for 5 minutes to obtain granulation liquid; S3: Preparation of continuous phase: Mix 240kg of water and 1kg of long-acting fungicide at a speed of 500r / min, then add 25kg of nanocellulose and 1kg of Plus330 hydrophobically modified cellulose and stir for 5-10min, then add 25kg of ethylene glycol, 25kg of film-forming aid, and 1kg of multifunctional aid, adjust the speed to 1300r / min and stir and disperse for 10min, then adjust the speed to 600r / min, add 430kg of RS-3799A emulsion, 180kg of RS-3765 emulsion, 2kg of rapid fungicide, 2kg of thickener, and 10kg of silica sol, stir and mix for 5 minutes to obtain a continuous phase S4: 550 kg of base paint and 200 kg of granulation liquid are mixed and granulated to obtain color particles; S5: Add 100 kg of the continuous phase into step S4, and stir and mix to obtain a water-in-sand coating.
[0028] Example 2 A method for preparing an anti-color seepage water-in-sand coating comprises the following steps: S1: Prepare the base paint S11: 4 kg of S482 protective glue was mixed with 36 kg of water, and dispersed at a speed of 1200 ± 10 r / min for 40 minutes to form a protective glue solution with a concentration of 10%; S12: 280kg of water, 1kg of long-acting fungicide, 2kg of dispersant and 2kg of defoamer are stirred and mixed at a speed of 300±10r / min, and then 6.5kg of titanium dioxide, 4kg of hydrophobically modified cellulose and 4kg of hydroxyethyl cellulose are added while stirring, and then the speed is adjusted to 500±10r / min, and stirring is continued for 5min, and then 12kg of ethylene glycol, 12kg of film-forming aid and 2kg of multifunctional aid are added, and then the speed is adjusted to 1300r / min and dispersed for 10 minutes; wherein the hydrophobically modified cellulose is composed of HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose in a weight ratio of 1:2; S13: Add 180 kg of acrylic emulsion to the solution obtained in step S12, reduce the rotation speed to 800 ± 10 r / min, and stir for 10 min; S14: squeeze the protective glue solution obtained in step S11, 2 kg of modified guar gum, and 2 kg of sodium tetraborate decahydrate into the solution obtained in step S13, and then adjust the speed to 1200±10 r / min and disperse for 10 min; S15: Add 2 kg of defoamer, 2 kg of quick bactericide, 0.1 kg of wetting agent and 450 kg of 80-120 mesh calcined colored sand to the solution obtained in step S14 to obtain a base paint; S2: Preparation of granulation liquid: 500 kg of water and 2 kg of long-acting fungicide were stirred and mixed evenly, 25 kg of S80 protective glue, 1 kg of xanthan gum and 1 kg of carboxymethyl cellulose were added at a speed of 800 ± 10 r / min, and after dispersion for 5 minutes, 1 kg of multifunctional auxiliary agent was added, and the speed was adjusted to 1300 r / min. After dispersion for 35 minutes, 1 kg of rapid fungicide and 500 kg of water were added, and the speed was adjusted to 400 r / min and dispersed for 5 minutes to obtain a granulation liquid; S3: Preparation of continuous phase: 250kg of water and 1kg of long-acting fungicide were mixed at a speed of 500r / min, and then 30kg of nanocellulose and 1kg of Plus330 hydrophobically modified cellulose were added and stirred for 5min, and then 30kg of ethylene glycol, 30kg of film-forming aid, and 1kg of multifunctional aid were added. The speed was adjusted to 1300r / min and stirred and dispersed for 10min. After the speed was adjusted to 600r / min, 450kg of RS-3799A emulsion, 200kg of RS-3765 emulsion, 3kg of rapid fungicide, 2kg of thickener, and 20kg of silica sol were added, and a continuous phase was obtained after stirring and mixing for 5 minutes. S4: 600 kg of base paint and 250 kg of granulation liquid are mixed and granulated to obtain color particles; S5: Add 150 kg of continuous phase to step S4, and stir and mix to obtain water-in-sand coating.
[0029] Example 3 A method for preparing an anti-color seepage water-in-sand coating comprises the following steps: S1: Prepare the base paint S11: 5 kg of S482 protective glue was mixed with 45 kg of water, and dispersed at a speed of 1200 ± 10 r / min for 40 minutes to form a protective glue solution with a concentration of 10%; S12: 291kg water, 1.7kg long-acting fungicide, 3kg dispersant, and 2.5kg defoamer are stirred and mixed at a speed of 300±10r / min, and then 8kg titanium dioxide, 5kg hydrophobically modified cellulose, and 5kg hydroxyethyl cellulose are added while stirring, and then the speed is adjusted to 500±10r / min, and stirring is continued for 10min, and then 14kg ethylene glycol, 15kg film-forming aid, and 2kg multifunctional aid are added, and then the speed is adjusted to 1300r / min for dispersion for 15 minutes; wherein the hydrophobically modified cellulose is composed of HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose in a weight ratio of 1:2; S13: Add 200 kg of acrylic emulsion to the solution obtained in step S12, reduce the rotation speed to 800 ± 10 r / min, and stir for 10 min; S14: squeeze the protective glue solution obtained in step S11, 3 kg of modified guar gum, and 3 kg of sodium tetraborate decahydrate into the solution obtained in step S13, and then adjust the speed to 1200±10 r / min and disperse for 10 min; S15: Add 2.5 kg of defoamer, 3.3 kg of quick bactericide, 0.2 kg of wetting agent and 460 kg of 80-120 mesh calcined colored sand to the solution obtained in step S14 to obtain a base paint; S2: Preparation of granulation liquid: 500 kg of water and 2 kg of long-acting fungicide were stirred and mixed evenly, 30 kg of S80 protective glue, 2 kg of xanthan gum and 1.5 kg of carboxymethyl cellulose were added at a speed of 800 ± 10 r / min, and after dispersion for 5 minutes, 2 kg of multifunctional auxiliary agent was added, and the speed was adjusted to 1300 r / min. After dispersion for 35 minutes, 2 kg of rapid fungicide and 500 kg of water were added, and the speed was adjusted to 400 r / min and dispersed for 5 minutes to obtain granulation liquid; S3: Preparation of continuous phase: 260kg of water and 2kg of long-acting fungicide were mixed at a speed of 500r / min, and then 35kg of nanocellulose and 2kg of Plus330 hydrophobically modified cellulose were added and stirred for 10min, and then 35kg of ethylene glycol, 35kg of film-forming aid, and 2kg of multifunctional aid were added. The speed was adjusted to 1300r / min and stirred and dispersed for 10min. After the speed was adjusted to 600r / min, 460kg of RS-3799A emulsion, 220kg of RS-3765 emulsion, 4kg of rapid fungicide, 3kg of thickener, and 50kg of silica sol were added, and the continuous phase was obtained after stirring and mixing for 10 minutes. S4: 650 kg of base paint and 300 kg of granulation liquid are mixed and granulated to obtain color particles; S5: Add 200 kg of continuous phase to step S4, and stir and mix to obtain water-in-sand coating.
[0030] Example 4 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 2 in that an equal amount of modified guar gum obtained in Preparation Example 1 is used in step S14, and the rest is the same as that of Example 2.
[0031] Example 5 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 2 in that an equal amount of modified guar gum obtained in Preparation Example 2 is used in step S14, and the rest is the same as that of Example 2.
[0032] Example 6 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 4 in that an equal amount of calcined colored sand obtained in Preparation Example 3 is used in step S15, and the rest is the same as that of Example 4.
[0033] Example 7 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 4 in that an equal amount of calcined colored sand obtained in Preparation Example 4 is used in step S15, and the rest is the same as that of Example 4.
[0034] Example 8 A method for preparing an anti-colorization water-coated sand coating is different from Example 7 in that silica sol is not added to the continuous phase, and the rest is the same as Example 7.
[0035] Comparative Example 1 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 7 in that modified guar gum and sodium tetraborate decahydrate are not included in step S14, and the rest is the same as that of Example 7.
[0036] Comparative Example 2 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 7 in that no modified guar gum is included in step S14, and the rest is the same as that of Example 7.
[0037] Comparative Example 3 A method for preparing an anti-colorization water-coated sand coating, which is different from Example 7 in that sodium tetraborate decahydrate is used in step S14, and the rest is the same as Example 7.
[0038] Comparative Example 4 A method for preparing an anti-colorization water-coated sand coating is different from that of Example 7 in that an equal amount of guar gum replaces modified guar gum in step S14.
[0039] Performance Testing The water-in-sand coatings obtained in the above embodiments and comparative examples were tested for adhesion and washability. The water-in-sand coatings obtained in the above embodiments and comparative examples were sprayed onto a test plate using a spray gun with a pressure of 0.5 MPa to see whether broken particles would occur. The test results are shown in Table 1.
[0040] The washability is tested in accordance with the relevant provisions of HG / T4343-2012 "Water-based Multi-color Architectural Coatings"; The adhesion test is carried out in accordance with the relevant provisions of GB / T9286-1998 "Scratch test for paint and varnish films", with grade 0 being the best and grade 5 being the worst.
[0041] Table 1 Test results of water-based sand coating From the table above we can see that: The water-based sand coating obtained in the examples of the present application has good adhesion to the substrate, and the number of wash resistance is more than 10,000. After spraying with a pressure of 0.5 MPa, no broken particles appear, indicating that the color particles of the present application have good toughness and the paint film surface also has excellent strength.
[0042] Compared with Example 7, when the base paint lacks modified guar gum and sodium tetraborate decahydrate or lacks guar gum or lacks sodium tetraborate decahydrate, the adhesion grade of the paint film is correspondingly reduced, and after being sprayed onto the test plate, the color particles appear broken, indicating that the color particles in the water-based sand coatings obtained in Comparative Examples 1-3 have poor toughness and the number of washing resistance is also significantly reduced, indicating that the surface strength of the paint film is reduced compared with Example 7.
[0043] Compared with Example 7, when guar gum was used instead of modified guar gum in Comparative Example 4, the color particles did not break after spraying, but the washability of the paint film was significantly reduced compared with that of Example 7, indicating that the surface strength of the paint film was reduced compared with that of Example 7.
[0044] The embodiments of this specific implementation method are all preferred embodiments of the present invention, and are not intended to limit the protection scope of the present invention. Therefore, any equivalent changes made based on the structure, shape, and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. An anti-color seepage water-in-sand coating, characterized in that , including the following raw materials in parts by weight: 550-650 parts of base paint, 200-300 parts of granulation liquid, 100-200 parts of continuous phase, the base paint includes 296-336 parts of water, 2-5 parts of fungicide, 1-3 parts of dispersant, 5-8 parts of titanium dioxide, 3-5 parts of defoamer, 3-5 parts of hydrophobically modified cellulose, 4-5 parts of hydroxyethyl cellulose, 10-14 parts of ethylene glycol, 10-15 parts of film-forming aid, 1-2 parts of multifunctional additive, 160-200 parts of acrylic emulsion, 3-5 parts of S482 protective glue, 0.1-0.2 parts of wetting agent, 420-460 parts of 80-120 mesh calcined colored sand, 1-3 parts of modified guar gum, and 1-3 parts of sodium tetraborate decahydrate; The bactericide consists of a DMB long-acting bactericide and a HF fast bactericide.
2. The anti-color seepage water-in-sand coating according to claim 1, characterized in that: The modified guar gum is obtained by the following preparation method: S1: 35-45g of tetraethylene glycol is dissolved in 50ml of tetrahydrofuran, 8-12g of sodium hydroxide is dissolved in 60ml of water to form a sodium hydroxide aqueous solution, the tetrahydrofuran solution containing tetraethylene glycol and the sodium hydroxide aqueous solution are mixed under ice bath conditions, and then tetrahydrofuran dissolved with toluene-4-sulfonyl chloride is added dropwise, the reaction is stirred in the ice bath for 3-4 hours, the reaction solution obtained by the reaction is extracted with dichloromethane, and then water is removed and suction filtered to obtain an activated tetraethylene glycol solution; S2: 2-3 g of guar gum is added to 3-4 g of isopropanol and stirred. After adding 0.3-0.5 g of sodium hydroxide at a temperature of 25-30° C. for alkalization for 20-30 minutes, the activated tetraethylene glycol solution obtained in step S1 is added under a temperature of 50-55° C. and reacted for 3-5 hours. The modified guar gum is filtered and dried.
3. The anti-color seepage water-in-sand coating according to claim 1 or 2, characterized in that: The calcined colored sand is obtained by the following preparation method: S1: adding 3-5 parts by weight of a pigment to 15-25 parts by weight of an aqueous solution containing 10-20 wt% of an aqueous hyperdispersant, and obtaining a pigment paste by ultrasonic dispersion; S2: Add 8-10 parts by weight of aluminum dihydrogen phosphate and 0.3-0.5 parts by weight of boric acid into 100 parts by weight of quartz sand, then add the pigment paste obtained in step S1, stir evenly, and calcine at 600-700° C. for 3-5 hours to obtain calcined colored sand.
4. The anti-color seepage water-in-sand coating according to claim 1, characterized in that: The hydrophobically modified cellulose includes HE-10K hydrophobically modified cellulose and HM-10K hydrophobically modified cellulose in a weight ratio of 1:
2.
5. The anti-color seepage water-in-sand coating according to claim 1, characterized in that: The granulation liquid comprises, by weight, 1000 parts of water, 1-2 parts of long-acting fungicide, 20-30 parts of S80 protective glue, 1-2 parts of xanthan gum, 1-1.5 parts of carboxymethyl cellulose, 1-2 parts of multifunctional auxiliary agent and 1-2 parts of rapid fungicide.
6. The anti-color seepage water-in-sand coating according to claim 5, characterized in that: The continuous phase comprises, by weight, 240-260 parts of water, 1-2 parts of long-acting bactericide, 25-35 parts of nanocellulose, 1-2 parts of Plus330 hydrophobically modified cellulose, 25-35 parts of ethylene glycol, 25-35 parts of film-forming aid, 1-2 parts of multifunctional aid, 430-460 parts of RS-3799A emulsion, 180-220 parts of RS-3765 emulsion, 2-4 parts of rapid bactericide, 2-3 parts of thickener, and 10-30 parts of silica sol.
7. A method for preparing the anti-color seepage water-in-sand coating according to any one of claims 1 to 6, characterized in that: The steps include: S1: Prepare the base paint S11: Mix S482 protective glue with part of water, and disperse for 40-50 minutes at a rotation speed of 1200±10r / min to form a protective glue solution with a concentration of 10%; S12: Stir and mix the remaining water, long-acting fungicide, dispersant and defoamer at a speed of 300±10r / min, then add titanium dioxide, hydrophobically modified cellulose and hydroxyethyl cellulose while stirring, then adjust the speed to 500±10r / min, continue stirring for 5-10min, then add ethylene glycol, film-forming aid and multifunctional aid, then adjust the speed to 1300r / min and disperse for 5-15 minutes; S13: Add acrylic emulsion to the solution obtained in step S12, lower the speed to 800±10r / min, and stir for 5-10min; S14: squeeze the protective glue solution, modified guar gum and sodium tetraborate decahydrate obtained in step S11 into the solution obtained in step S13, and then adjust the speed to 1200±10r / min for dispersion for 5-10min; S15: adding a rapid bactericide, a wetting agent and calcined colored sand to the solution obtained in step S14 to obtain a base paint; S2: mixing the base paint and the granulation liquid to obtain color particles; S3: Add the continuous phase to step S2, and stir and mix to obtain the water-in-sand coating.
8. The method for preparing the anti-color seepage water-in-sand coating according to claim 7, characterized in that: The granulation liquid is prepared as follows: by weight, 500 parts of water and 1-2 parts of long-acting fungicide are stirred and mixed uniformly, 20-30 parts of S80 protective glue, 1-2 parts of xanthan gum, and 1-1.5 parts of carboxymethyl cellulose are added at a rotation speed of 800±10 r / min, and after dispersion for 5-10 minutes, 1-2 parts of multifunctional auxiliary agent are added, the rotation speed is adjusted to 1300 r / min, and after dispersion for 35-45 minutes, 1-2 parts of rapid fungicide and 500 parts of water are added, and the rotation speed is adjusted to 400 r / min and dispersion is carried out for 5 minutes to obtain the granulation liquid.
9. The method for preparing the anti-color seepage water-in-sand coating according to claim 8, characterized in that: The continuous phase is prepared by mixing 240-260 parts of water and 1-2 parts of long-acting fungicide by weight at a rotation speed of 500 r / min, then adding 25-35 parts of nanocellulose and 1-2 parts of hydrophobically modified cellulose, stirring and mixing for 5-10 minutes, then adding 25-25 parts of ethylene glycol, 25-35 parts of film-forming aids, and 1-2 parts of multifunctional aids, adjusting the rotation speed to 1300 r / min and stirring and dispersing for 10-20 minutes, then adjusting the rotation speed to 600 r / min, adding 430-460 parts of RS-3799A emulsion, 180-220 parts of RS-3765 emulsion, 2-4 parts of rapid fungicide, 2-3 parts of thickener, and 10-30 parts of silica sol, stirring and mixing for 5-10 minutes to obtain a continuous phase.
Citation Information
Patent Citations
Formula and process for crosslinking antimicrobials to surfaces and polymers
CA2922468A1
Preparation method of organic polymer MOPPV (Poly(2,5-dimethoxy p-phenylene Vinylene)) / PbSe nanocrystal composite material
CN103172835A
Dabigatran etexilate analog centered by fluorine-containing-group-modified benzene ring and synthesis method thereof
CN103694178A
Sand in water thermal-insulation colorful paint, and preparation method thereof
CN108912903A
Amphiphilic molecule containing o-nitrobenzyl ester photo-degradation group
CN110003031A