Multi-angle soft light finishing varnish with uniform gloss and no floating and preparation method thereof

By preparing a soft-gloss finish varnish with uniform gloss and no blooming at multiple angles, the problem of roller marks and uneven gloss when the soft-gloss finish is applied to latex paint is solved, and excellent leveling and high transparency are achieved, satisfying the needs of Consumer demand for wall beauty and protection.

CN118755326APending Publication Date: 2024-10-11BEIXIN JIABAOLI COATINGS (GUANGDONG) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410826218.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-24
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Most of the soft-gloss varnishes on the market are prone to roller marks and uneven side gloss after application on latex paint substrates, resulting in poor visual effects, and the problem of uneven gloss caused by uneven walls is difficult to solve. .

Method used

Use a soft-gloss finish varnish with uniform gloss and no blooming from multiple angles, by combining water, antifreeze, pH regulator, defoaming agent, film-forming aid, high Tg emulsion, matting emulsion, bactericide, preservative and association Type alkali swelling thickener and leveling agent, through the stirring step, a paint film with excellent leveling and high transparency is prepared, and the surface tension and shear viscosity are controlled to achieve uniform gloss and stain resistance.

Benefits of technology

It achieves the reduction of roller marks and uniform gloss during construction on latex paint, improves the visual effect, and provides good stain resistance and high transparency to meet consumers' needs for wall beauty and protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755326A_ABST
    Figure CN118755326A_ABST
Patent Text Reader

Abstract

The invention relates to multi-angle soft light finishing varnish with uniform gloss and no floating and a preparation method of the soft light finishing varnish, and relates to the technical field of varnish preparation. The multi-angle soft light finishing varnish with uniform gloss and no floating is prepared from the following raw materials in parts by weight: 30 to 60 parts of water, 0.5 to 1.5 parts of an anti-freezing agent, 0.1 to 0.2 part of a pH (Potential of Hydrogen) regulator, 0.1 to 0.5 part of a de-foaming agent, 1.0 to 4.0 parts of a coalescing agent, 25 to 40 parts of high Tg emulsion, 10 to 30 parts of extinction emulsion, 0.2 to 0.3 part of a sterilizing agent and 0.2 to 0.6 part of a preservative, and 0-1.5 parts by weight of an associative alkali swelling thickener mixed with water, and the like. The invention solves the problems of floating phenomenon of non-uniform glossiness during construction due to poor wall flatness of the existing emulsion paint eggshell light product, and roller mark phenomenon during roller coating due to poor leveling property of the cover surface, and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of varnish preparation, in particular to a multi-angle, uniform, non-blooming soft-light cover varnish and a preparation method thereof. Background Art

[0002] As people's living standards continue to improve, more and more consumers have increasingly stringent requirements for home wall decoration. Consumers have gradually developed requirements for wall stain resistance, hardness, gloss and other properties. Therefore, in order to keep the latex paint wall clean and beautiful for a long time, consumers often apply soft gloss topcoat varnish on the latex paint to play a role in long-term protection and beauty. The most popular soft gloss topcoat varnish on the market (the soft light in this patent refers to the 60° gloss between 10 and 30), but most of the soft gloss topcoat varnish on the market will appear roller marks when observed from the side after rolling on the latex paint substrate and drying, and often due to the unevenness of the substrate, the side gloss will be uneven, which will appear visually abrupt and greatly affect the visual effect. At the same time, for consumers who have been decorating with matte gloss latex paint for several years, they will gradually become aesthetically fatigued with the wall. Most consumers also hope to directly improve the wall gloss and better protect the wall on the original basis, giving it a more active and comfortable range.

[0003] In view of this, there is an urgent need to develop a soft light topcoat varnish with better performance to better meet the consumer's use needs and construction requirements. Summary of the invention

[0004] The invention provides a multi-angle soft-light top varnish with uniform gloss and no blooming and a preparation method thereof, which can solve the problem of uneven gloss and blooming during construction of current latex paint eggshell gloss products due to poor wall flatness, and solve the problem of roller marks on the top surface due to poor leveling when rolling. The top surface has good leveling, uniform gloss, smooth hand feel, etc., and at the same time, the top surface has good stain resistance and high transparency.

[0005] In a first aspect, the present invention provides a multi-angle uniform gloss and non-blooming soft light top varnish, wherein the multi-angle uniform gloss and non-blooming soft light top varnish comprises the following raw materials in parts by weight:

[0006] 30-60 parts by weight of water, 0.5-1.5 parts by weight of antifreeze agent, 0.1-0.2 parts by weight of pH regulator, 0.1-0.5 parts by weight of defoamer, 1.0-4.0 parts by weight of film-forming aid, 25-40 parts by weight of high Tg emulsion, 10-30 parts of matte emulsion, 0.2-0.3 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0-1.5 parts by weight of associative alkali swelling thickener diluted with water and 0.3-0.5 parts by weight of leveling agent.

[0007] Furthermore, the multi-angle glossy, uniform, non-blooming soft-light top varnish comprises the following raw materials, in parts by weight: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 25 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

[0008] Furthermore, the multi-angle glossy, uniform, non-blooming soft-light top varnish comprises the following raw materials, in parts by weight: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 20 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

[0009] Furthermore, the multi-angle gloss uniform and non-blooming soft-light top varnish comprises the following raw materials, in parts by weight: 31.95 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 30 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water and 1.5 parts by weight of leveling agent.

[0010] Furthermore, the multi-angle glossy and uniform non-blooming soft light top varnish comprises the following raw materials in parts by weight:

[0011] 42.15 parts by weight of water, 1 part by weight of antifreeze agent, 0.1 part by weight of pH regulator, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 30 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.3 parts by weight of associative alkali swelling thickener diluted with water and 1.1 parts by weight of leveling agent.

[0012] Furthermore, the associative alkali swelling thickener after adding water is compounded by water and the associative alkali swelling thickener in a weight ratio of (3-10):1.

[0013] Furthermore, the product model of the high Tg emulsion is Wanhua Chemical Group Co., Ltd. 8055 silicon-modified acrylic emulsion, the product model of the matte emulsion is EM-5233 emulsion of Jiangmen Jinqiao New Materials Co., Ltd.

[0014] In a second aspect, the present invention provides a method for preparing the multi-angle gloss uniform and non-blooming soft light top varnish according to any one of the first aspects, the preparation method comprising the following steps:

[0015] The water, the antifreeze agent, the pH regulator, the defoaming agent and the film-forming aid are first stirred to obtain a first mixture;

[0016] Adding high Tg emulsion and matte emulsion to the first mixed material and performing a second stirring to obtain a second mixed material;

[0017] Add a bactericide, a preservative, an associative alkali swelling thickener and a leveling agent diluted with water to the second mixture for a second stirring to obtain the multi-angle glossy, uniform, non-blooming soft-gloss top varnish.

[0018] Furthermore, the working parameters of the first stirring include: 250-350r / min; the working parameters of the second stirring include: 250-350r / min; the working parameters of the third stirring include: the speed after adding the associative alkali swelling thickener diluted with water is 450-500r / min, and the speed after adding the leveling agent is 800-900r / min.

[0019] The above technical solution provided by the embodiment of the present invention has at least the following advantages compared with the prior art:

[0020] The present invention provides a multi-angle uniform gloss non-blooming soft light top varnish and a preparation method thereof. Through the mutual cooperation of various components, the joint action can solve the problem of uneven gloss and blooming during construction of current latex paint eggshell gloss products due to poor wall flatness, and solve the problem of roller marks during rolling due to poor leveling of the top surface. The top surface has good leveling, uniform gloss, smooth hand feel, etc., and the top surface has good stain resistance and high transparency. Specifically:

[0021] 1) It can achieve excellent leveling performance and solve the problem of roller marks easily appearing when soft light cover is constructed on latex paint.

[0022] 2) A “uniform” 60-degree and 85-degree gloss can be obtained on the surface, solving the problem of uneven gloss caused by uneven walls.

[0023] 3) The multi-angle, uniform, non-blooming soft-light top varnish provided by the present invention solves the problems raised in the above-mentioned background technology and meets the usage needs of consumers. While ensuring high transparency, stain resistance and hardness, it also has better leveling performance, smooth feel and uniform and soft side gloss, and can obtain good visual effects.

[0024] 4) The paint film of the present invention has excellent leveling performance, so that the paint film is leveled and smooth on the surface of the substrate, actively weakening or even eliminating the roller edge mark, so that the drying process is fully uniform. In the coating system, the leveling of the wet film after rolling can be controlled by controlling the low shear (Brookfield) viscosity and the size of the surface tension, because the surface tension and gravity are the main forces that promote the flow and leveling of the coating film, and the structural characteristics of the low shear viscosity are the main forces that hinder the leveling of the paint film. Therefore, the lower the low shear viscosity, the better the wet film after rolling on the substrate. The lower the internal movement resistance, the more conducive it is to the flow and leveling of the wet film on the substrate. The higher the surface tension, the easier it is for the wet film to level, and the shorter the time. The topcoat varnish belongs to a water-based system, and the overall viscosity will gradually increase with the evaporation of water. In order to take into account the use in a variety of temperature and humidity environments and different water absorption capacities of substrates, the topcoat varnish should have a faster leveling ability, that is, the shorter the time it takes to level to a certain degree, the better. Therefore, the topcoat needs to have a larger surface tension and a lower low-shear viscosity. At the same time, in order to maintain the fullness of the paint film, its low-shear viscosity will gradually increase to prevent sagging.

[0025] 5) In the present invention, the difference in the glossiness of the paint film from 60° to 85° is reduced and the glossiness of the entire glossiness area is "uniformed". The specific numerical difference is less than 2, but the numerical value is between 10 and 30, so as to obtain the "uniform" glossiness of the paint film between the observation angle of 60° and 85°. The surface roughness structure of the paint film can be changed to form a special surface "uniform" structure, so that the gloss of the light reflected at the incident angle of 60 to 85 degrees is "uniform". Small particle size emulsion and matte emulsion can be used in combination, so that a uniform "uniform" structure is formed on the surface of the paint film during the film formation process, thereby changing the surface structure of the paint film. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the invention and, together with the description, serve to explain the principles of the invention.

[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0028] Figure 1 This is the actual effect picture showing that during the drying process of the existing soft light cover varnish, the drying time on both sides of the roller print is much longer than that in the middle.

[0029] Figure 2 This is a schematic diagram of the wavy structure of the existing soft-light top coat varnish which makes the top coat on the base material microscopically uneven.

[0030] Figure 3 This is the actual effect of the unevenness and defects on the wall when light is shining from the side.

[0031] Figure 4 Schematic diagram of the visual blurring phenomenon when looking sideways in the direction of light.

[0032] Figure 5 This is the light reflection diagram on the flat wall ( Figure 5 Middle left) and light reflection on uneven wall ( Figure 5 (center right)

[0033] Figure 6 A flow chart of a method for preparing a multi-angle, uniform, non-blooming soft-light top varnish provided by an embodiment of the present invention.

[0034] Figure 7 This is the actual effect of the commercially available soft light cover spray.

[0035] Figure 8 This is the actual effect diagram of the roller coating of Comparative Example 3. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0038] As people's living standards improve, more and more consumers have increasingly stringent requirements for home wall decoration, and gradually have requirements for wall resistance, hardness and other properties. Therefore, in order to keep the latex paint walls clean and beautiful for a long time, consumers often apply topcoat varnish on latex paint to play a long-term protective role. Currently, the most popular on the market is soft gloss topcoat varnish (the soft light in this patent refers to a 60° gloss between 10 and 30), but most of the soft gloss topcoat varnish on the market is rolled on the latex paint substrate and left to dry. When observed from the side, roller marks will appear, and often due to the unevenness of the substrate, the side gloss will be uneven, which will appear visually abrupt and greatly affect the visual effect.

[0039] The inventor has found that there are two main reasons for the above problems. One is that the leveling of the finish is not good and the glossiness of the finish paint film at different angles is very different. When rolling, the two sides of the roller are very easy to pile up. Although the overall wall surface is relatively uniform when wet overlapped, the thickness of the wet film is actually different. When the material is thick, it is thick, and when the material is thin, it is thin. The piled-up material on both sides of the roller print leads to a wavy microstructure, which is specifically manifested in the drying process. The drying time on both sides of the roller print is much longer than that in the middle (such as Figure 1 ), so that the surface of the substrate is uneven and the stacking position is wavy, such as Figure 2 The glossiness is higher in thick areas and lower in thin areas. The second is the unevenness of the wall itself (such as Figure 3 As shown in the figure, the glossiness of the topcoat film varies greatly at different angles. When the wall is uneven, the incident angle of light is different from the angles of the other walls. Since the glossiness of the topcoat at different angles is different, there is a visually obvious gloss difference, which gives a visual blurring phenomenon when looking sideways in the direction of light, such as Figure 4 shown.

[0040] The gloss on the paint film surface will change gradually with the change of the incident angle of light. If the wall is flat, then the wall will change from bright gloss to dull gloss when viewed from the side, which is continuous and not abrupt. However, when the wall is uneven, the gloss reflection angle before and after the uneven point is not gradual but sudden, so the gloss change at the uneven point is not gradual but rapid, thus forming a visual gloss abruptness, such as Figure 5 shown.

[0041] In order to solve the above problems / achieve the above technical effects, the technical solutions provided by the present invention are as follows:

[0042] In a first aspect, the present invention provides a multi-angle uniform gloss and non-blooming soft light top varnish, wherein the multi-angle uniform gloss and non-blooming soft light top varnish comprises the following raw materials in parts by weight:

[0043] 30-60 parts by weight of water, 0.5-1.5 parts by weight of antifreeze agent, 0.1-0.2 parts by weight of pH regulator, 0.1-0.5 parts by weight of defoamer, 1.0-4.0 parts by weight of film-forming aid, 25-40 parts by weight of high Tg emulsion, 10-30 parts of matte emulsion, 0.2-0.3 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0-1.5 parts by weight of associative alkali swelling thickener diluted with water and 0.3-0.5 parts by weight of leveling agent.

[0044] The present invention provides a multi-angle uniform gloss non-blooming soft light top varnish and a preparation method thereof. Through the mutual cooperation of various components, the joint action can solve the problem of uneven gloss and blooming during construction of current latex paint eggshell gloss products due to poor wall flatness, and solve the problem of roller marks during rolling due to poor leveling of the top surface. The top surface has good leveling, uniform gloss, smooth hand feel, etc., and the top surface has good stain resistance and high transparency. Specifically:

[0045] 1) It can achieve excellent leveling performance and solve the problem of roller marks easily appearing when soft light cover is constructed on latex paint.

[0046] 2) A “uniform” 60-degree and 85-degree gloss can be obtained on the surface, solving the problem of uneven gloss caused by uneven walls.

[0047] 3) The multi-angle, uniform, non-blooming soft-light top varnish provided by the present invention solves the problems raised in the above-mentioned background technology and meets the usage needs of consumers. While ensuring high transparency, stain resistance and hardness, it also has better leveling performance, smooth feel and uniform and soft side gloss, and can obtain good visual effects.

[0048] 4) The paint film of the present invention has excellent leveling performance, so that the paint film is leveled and smooth on the surface of the substrate, actively weakening or even eliminating the roller edge mark, so that the drying process is fully uniform. In the coating system, the leveling of the wet film after rolling can be controlled by controlling the low shear (Brookfield) viscosity and the size of the surface tension, because the surface tension and gravity are the main forces that promote the flow and leveling of the coating film, and the structural characteristics of the low shear viscosity are the main forces that hinder the leveling of the paint film. Therefore, the lower the low shear viscosity, the better the wet film after rolling on the substrate. The lower the internal movement resistance, the more conducive it is to the flow and leveling of the wet film on the substrate. The higher the surface tension, the easier it is for the wet film to level, and the shorter the time. The topcoat varnish belongs to a water-based system, and the overall viscosity will gradually increase with the evaporation of water. In order to take into account the use in a variety of temperature and humidity environments and different water absorption capacities of substrates, the topcoat varnish should have a faster leveling ability, that is, the shorter the time it takes to level to a certain degree, the better. Therefore, the topcoat needs to have a larger surface tension and a lower low-shear viscosity. At the same time, in order to maintain the fullness of the paint film, its low-shear viscosity will gradually increase to prevent sagging.

[0049] 5) In the present invention, the difference in the glossiness of the paint film from 60° to 85° is reduced and the glossiness of the entire glossiness area is "uniformed". The specific numerical difference is less than 2, but the numerical value is between 10 and 30, so as to obtain the "uniform" glossiness of the paint film between the observation angle of 60° and 85°. The surface roughness structure of the paint film can be changed to form a special surface "uniform" structure, so that the gloss of the light reflected at the incident angle of 60 to 85 degrees is "uniform". Small particle size emulsion and matte emulsion can be used in combination, so that a uniform "uniform" structure is formed on the surface of the paint film during the film formation process, thereby changing the surface structure of the paint film.

[0050] In some specific embodiments, the multi-angle gloss uniform and non-blooming soft-light top varnish includes the following raw materials, measured in parts by weight: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 25 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

[0051] In some specific embodiments, the multi-angle gloss uniform and non-blooming soft-light top varnish includes the following raw materials, measured in parts by weight: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 20 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

[0052] In some specific embodiments, the multi-angle gloss uniform and non-blooming soft-light top varnish includes the following raw materials, measured in parts by weight: 31.95 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 30 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

[0053] In some specific embodiments, the multi-angle glossy and non-blooming soft light top varnish comprises the following raw materials in parts by weight:

[0054] 42.15 parts by weight of water, 1 part by weight of antifreeze agent, 0.1 part by weight of pH regulator, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 30 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.3 parts by weight of associative alkali swelling thickener diluted with water and 1.1 parts by weight of leveling agent.

[0055] In some specific embodiments, the associative alkali swelling thickener after adding water is compounded by water and associative alkali swelling thickener in a weight ratio of (3-10):1.

[0056] In some specific embodiments, the product model of the high Tg emulsion is Wanhua Chemical Group Co., Ltd. 8055 silicon-modified acrylic emulsion, the product model of the matte emulsion is EM-5233 emulsion of Jiangmen Jinqiao New Materials Co., Ltd.

[0057] It should be noted that the components and raw materials involved in the multi-angle gloss uniform and non-blooming soft-gloss topcoat varnish provided by the present invention can all be commercially available products unless otherwise specified or specifically stated. For example, the preferred antifreeze agent is ethylene glycol, the preferred pH adjuster is Dow's AMP-95, the matte emulsion is the EM-5233 emulsion of Jiangmen Jinqiao New Materials Co., Ltd., which is characterized by a glossiness at an angle of 85 degrees lower than that at an angle of 60 degrees, and the other matte emulsions added to the varnish have a glossiness at an angle of 85 degrees higher than that at an angle of 60 degrees; the small-particle high Tg emulsion is the 8055 silicon-modified acrylic emulsion, the preferred defoamer is DAPROAP 7010 from Hemmings, the preferred film-forming aid is COASOL from Dow, the preferred preservative is GT50 from Sol, the preferred non-associative alkali swelling thickener is RHEOLATE 185 from Hemmings, and the preferred leveling agent is RHEOLATE 602 from Hemmings.

[0058] In a second aspect, based on the same inventive concept, the present invention provides a method for preparing a soft light top varnish having uniform gloss at multiple angles and without blurring as described in any one of the first aspects, such as Figure 6 As shown, the preparation method comprises the following steps:

[0059] The water, the antifreeze agent, the pH regulator, the defoaming agent and the film-forming aid are first stirred to obtain a first mixture;

[0060] Adding high Tg emulsion and matte emulsion to the first mixed material and performing a second stirring to obtain a second mixed material;

[0061] Add a bactericide, a preservative, an associative alkali swelling thickener and a leveling agent diluted with water to the second mixture for a second stirring to obtain the multi-angle glossy, uniform, non-blooming soft-gloss top varnish.

[0062] The method for preparing the multi-angle uniform gloss and non-blooming soft-light top varnish provided by the embodiment of the present invention is simple to operate, does not require additional specific operating equipment, and is suitable for mass industrial production.

[0063] In some specific embodiments, the working parameters of the first stirring include: 250-350r / min; the working parameters of the second stirring include: 250-350r / min; the working parameters of the third stirring include: the speed after adding the associative alkali swelling thickener diluted with water is 450-500r / min, and the speed after adding the leveling agent is 800-900r / min.

[0064] It should be noted that in the preparation method of the multi-angle uniform gloss and non-blooming soft light top varnish provided by the present invention, unless there are special limitations or specific operating steps and process parameters, they can be carried out according to the existing coating preparation process, and the present invention will not go into details one by one.

[0065] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0066] The raw material product information involved in the following examples and comparative examples is as follows:

[0067] The antifreeze agent is preferably ethylene glycol;

[0068] The preferred pH adjuster is Dow's AMP-95;

[0069] The matte emulsion used is EM-5233 emulsion from Jiangmen Jinqiao New Materials Co., Ltd.

[0070] The small particle size high Tg emulsion is from Wanhua Chemical Group Co., Ltd. 8055 silicone modified acrylic emulsion;

[0071] The preferred defoamer is DAPROAP 7010 from Hemmings;

[0072] The preferred film-forming aid is COASOL from Dow;

[0073] The preferred preservative is Sol's GT50;

[0074] The non-associative alkali swelling thickener used is Hemmings' RHEOLATE 185;

[0075] The leveling agent selected is Hemmings' RHEOLATE 6025.

[0076] Embodiments 1 to 4 provide a multi-angle, uniform, non-blooming soft-light topcoat varnish, the production process of which is as follows:

[0077] Add 30-60 parts by weight of water into a dispersion tank, slowly add 0.5-1.5 parts by weight of antifreeze, 0.1-0.2 parts by weight of pH regulator, 0.1-0.5 parts by weight of defoamer, 1.0-4.0 parts by weight of film-forming aid under low-speed stirring at 250-350 r / min, slowly add 25-40 parts by weight of high Tg emulsion and 10-30 parts of matting emulsion after stirring for 3 minutes, add 0.2-0.3 parts by weight of fungicide and 0.2-0.6 parts by weight of preservative after stirring for 5 minutes, then add 0-1.0 parts by weight of associative alkali swelling thickener diluted with water at a ratio of 1:1, adjust the speed to 450-500 r / min, then slowly add 0.3-0.5 parts by weight of leveling agent, adjust the speed to 800-900 r / min, stir for 15 minutes and then discharge.

[0078] The specific weight parts of each component in Examples 1 to 4 are shown in Table 1.

[0079] Table 1

[0080]

[0081]

[0082] Comparative Example 1: Based on Example 1, 8055:5233=25:25 is changed to 20:30.

[0083] Comparative Example 2: Based on Example 1, 8055:5233=25:25 is changed to 35:35.

[0084] Comparative Example 3: Based on Example 1, RHEOLATE 6025 was reduced to 0 and RHEOLATE 185 was increased to 0.5.

[0085] Comparative Example 4: Based on Example 1, RHEOLATE 6025 was increased to 2, and RHEOLATE 185 was reduced to 0.1.

[0086] Comparative Example 5: Based on Example 1, an equal amount of the matte emulsion of the same particle size, Baolijia 9593, was used to replace 5233.

[0087] Comparative Example 6: Based on Example 2, 8055 and 5233 were replaced by equal amounts of Badful Matt Emulsion 8626.

[0088] Comparative Example 7: Based on Example 1, the ratio of small particle size high Tg emulsion (8055): matte emulsion (5233) = 25:25 was adjusted to 0:50, indicating that the glossiness at an angle of 60 degrees is relatively low and does not reach a soft gloss.

[0089] Test Case

[0090] In this example, the multi-angle gloss uniform and non-blooming soft-light topcoat varnish and commercially available products provided in the embodiments and comparative examples were subjected to performance tests, specifically including the following tests: 1) Viscosity: the viscosity of the topcoat was tested using a Stormer viscometer at 25±1°C; 2) Gloss: two coats of latex paint (specifically Carpoly 1918 eggshell gloss latex paint) were rolled on the smooth surface of the calcium silicate board. After it was completely dry, the first coat of topcoat varnish was applied on the latex paint using a mercerized master roller. After it was completely dry, the second coat of topcoat varnish was applied. After drying naturally for one day, the gloss was tested; 3) Gloss change rate: the absolute value of (85-degree angle gloss - 60-degree angle gloss) / 25; 4) Transparency: visually judged: a 150um wire rod was used to make a mold on a 5mm thick glass plate, which was placed in a 50°C oven and baked for 30 minutes. Place the side with the paint film on the textured substrate to observe whether it is varnished; 5) Watercolor pen resistance: after the sample prepared in 2) is cured at room temperature for 3 days, test the twelve watercolor pens under a wet rag for wiping immediately and wiping for 1 hour. After drying, observe whether there are marks. Compare and score with a full score of 10 and a pass of 6; 6) Rain mark resistance: after the sample prepared in 2) is cured at room temperature for 7 days, make the sample vertical to the horizontal plane, continue to drip water for 30 minutes, and observe the rain marks after the exposed water is completely dry; 7) Water whitening resistance: mold on the glass plate with a 100um wire rod, put it in a 50℃ oven for 2 hours after the surface is dry, take it out and leave it at room temperature for 2 hours, take it out after soaking in water for 4 hours, record the whitening degree and recovery time, the whitening degree can be divided into no whitening, slight whitening, slight whitening, whitening, and severe whitening.

[0091] The test results of each case are shown in Table 2 and Table 3.

[0092] Table 2 Performance test results of Examples 1 to 4 and Comparative Examples 1 and 7

[0093]

[0094]

[0095] Table 3 Comparative Examples 2 to 6 and Performance Test Results of Commercially Available Products

[0096]

[0097] In this example, large-scale construction tests were carried out on Example 1, Comparative Example 3, Comparative Example 5, Comparative Example 6 and commercially available products. The test results are shown in Table 4 and Figure 7 , Figure 8 As shown; Figure 7 This is the actual effect picture of the commercial soft light cover spray. The red frame is the abrupt gloss caused by the uneven wall, and the rest is uniform. Figure 8 This is the actual effect picture of roller coating of comparative example 3, and roller marks appear.

[0098] Table 4

[0099]

[0100]

[0101] In summary, the present invention provides a multi-angle uniform gloss soft-light top varnish and a preparation method thereof. Through the mutual coordination of various components, the joint action can solve the problem of uneven gloss and blooming during construction of current latex paint eggshell gloss products due to poor wall flatness, and at the same time solve the problem of roller marks on the top surface due to poor leveling when rolling. The top surface has good leveling, uniform gloss, smooth hand feel, etc. At the same time, the top surface has good stain resistance and high transparency.

[0102] Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present invention; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0103] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A multi-angle uniform gloss non-blooming soft light topcoat varnish, characterized in that: The multi-angle glossy and uniform non-blooming soft light topcoat varnish comprises the following raw materials in parts by weight: 30-60 parts by weight of water, 0.5-1.5 parts by weight of antifreeze agent, 0.1-0.2 parts by weight of pH regulator, 0.1-0.5 parts by weight of defoamer, 1.0-4.0 parts by weight of film-forming aid, 25-40 parts by weight of high Tg emulsion, 10-30 parts of matte emulsion, 0.2-0.3 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0-1.5 parts by weight of associative alkali swelling thickener diluted with water and 0.3-0.5 parts by weight of leveling agent.

2. The multi-angle glossy and non-blooming soft light top varnish according to claim 1, characterized in that: In parts by weight, the multi-angle glossy, uniform, and non-blooming soft-light top varnish comprises the following raw materials: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 25 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

3. The multi-angle gloss uniform and non-blooming soft light top varnish according to claim 1, characterized in that: In parts by weight, the multi-angle glossy, uniform, and non-blooming soft-light top varnish comprises the following raw materials: 41.85 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 20 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

4. The multi-angle uniform gloss non-blooming soft light top varnish according to claim 1, characterized in that: The multi-angle glossy, uniform, non-blooming soft-light top varnish comprises the following raw materials, in parts by weight: 31.95 parts by weight of water, 1 part by weight of antifreeze, 0.1 part by weight of pH adjuster, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 30 parts by weight of high Tg emulsion, 30 parts by weight of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.2 parts by weight of associative alkali swelling thickener diluted with water, and 1.5 parts by weight of leveling agent.

5. The multi-angle uniform gloss non-blooming soft light top varnish according to claim 1, characterized in that: The multi-angle glossy and uniform non-blooming soft light topcoat varnish comprises the following raw materials in parts by weight: 42.15 parts by weight of water, 1 part by weight of antifreeze agent, 0.1 part by weight of pH regulator, 0.3 part by weight of defoamer, 3.8 parts by weight of film-forming aid, 25 parts by weight of high Tg emulsion, 30 parts of matte emulsion, 0.25 parts by weight of bactericide, 0.2-0.6 parts by weight of preservative, 0.3 parts by weight of associative alkali swelling thickener diluted with water and 1.1 parts by weight of leveling agent.

6. The multi-angle uniform gloss non-blooming soft light top varnish according to any one of claims 1 to 5, characterized in that: The associative alkali swelling thickener after adding water is obtained by compounding water and the associative alkali swelling thickener in a weight ratio of (3-10):

1.

7. The multi-angle uniform gloss non-blooming soft light top varnish according to any one of claims 1 to 5, characterized in that: The product model of the high Tg emulsion is Wanhua Chemical Group Co., Ltd. 8055 silicon-modified acrylic emulsion, the product model of the matte emulsion is EM-5233 emulsion of Jiangmen Jinqiao New Materials Co., Ltd.

8. A method for preparing the multi-angle uniform gloss and non-blooming soft light top varnish according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: The water, the antifreeze agent, the pH regulator, the defoaming agent and the film-forming aid are first stirred to obtain a first mixture; Adding high Tg emulsion and matte emulsion to the first mixed material and performing a second stirring to obtain a second mixed material; Add a bactericide, a preservative, an associative alkali swelling thickener and a leveling agent diluted with water to the second mixture for a second stirring to obtain the multi-angle glossy, uniform, non-blooming soft-gloss top varnish.

9. The method for preparing the multi-angle uniform gloss non-blooming soft light top varnish according to claim 8, characterized in that: The working parameters of the first stirring include: 250-350r / min; the working parameters of the second stirring include: 250-350r / min; the working parameters of the third stirring include: the speed after adding the associative alkali swelling thickener diluted with water is 450-500r / min, and the speed after adding the leveling agent is 800-900r / min.

Citation Information

Patent Citations

  • Finishing paint and preparation method thereof

    CN107189670A

  • Ultra-matte single-component anti-doodling finishing varnish and preparation method thereof

    CN115612364A

  • Water-based reflective heat-insulating faux stone texture coating system for construction and preparation method thereof

    WO2017028471A1