Preparation process of anticorrosive paint added with fly ash

Through the composite process of nano-silica and epoxy acrylate and the use of fly ash as filler, the problems of high preparation cost and environmental pollution of anti-corrosion coatings are solved, efficient and low-cost reuse of fly ash is achieved, and the coating quality is improved. performance and environmental protection effects.

CN118755342AInactive Publication Date: 2024-10-11INNER MONGOLIA GUOYU TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410950586.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing anti-corrosion coating preparation process is complex and costly, resulting in environmental pollution and resource waste, and the utilization rate of fly ash is low. An effective process is needed to reduce costs and pollution and improve the utilization rate of fly ash.

Method used

Using the preparation and modification process of nano-silica, a high-performance water-based epoxy acrylate emulsion composite coating is prepared by combining different proportions of composite silicon sources with epoxy acrylate, and fly ash is added as a filler in the coating , utilizing its particle morphology and activity to improve coating performance.

Benefits of technology

It has reduced the cost of coatings, reduced environmental pollution, increased the comprehensive utilization of fly ash, improved the performance of coatings and the reuse rate of fly ash, and has dual economic and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755342A_ABST
    Figure CN118755342A_ABST
Patent Text Reader

Abstract

The invention provides a preparation process of an anti-corrosion coating added with fly ash. The preparation process of the anti-corrosion coating comprises the following steps: A, preparing nano silicon dioxide; b, modifying the nano silicon dioxide; c, preparing nano silicon dioxide from the composite silicon source in different proportions and modifying the nano silicon dioxide; d, preparing a nano silicon dioxide / epoxy acrylate composite coating; according to the invention, high value-added utilization of fly ash and energy conservation and emission reduction tasks are organically combined, so that not only is the comprehensive utilization approach of fly ash increased, but also the environmental pollution is reduced, the coating cost is reduced, and the method has double benefits in economic and social aspects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of anti-corrosion coating preparation, and in particular to a process for preparing anti-corrosion coating by adding fly ash. Background Art

[0002] As a major coal consumer and producer, my country is facing a series of environmental problems, such as large-scale land subsidence caused by coal mining. At the same time, the coal combustion process will produce huge waste resources. These fly ash pollutes the human environment greatly. Abandoned fly ash also occupies a large amount of land, causing land pollution. Therefore, in order to reduce its pollution to the human environment, fully increasing the use of fly ash, thereby improving or reducing the harm to the ecological environment of mines in multiple mining areas has become the focus of researchers. Countries around the world are actively looking for ways to comprehensively utilize fly ash, based on the differences in geographical location, coal quality, fly ash production, fly ash structural properties, and the development of process technology, environmental protection requirements, scarcity of raw materials, industrial structure and other factors.

[0003] In recent years, with the continuous development of society, people's living standards have been continuously improved, and therefore the requirements for living environment have become higher and higher. Social development means further development and utilization of resources, and the demand for coal has further increased. The accumulation of byproduct fly ash has further increased, and the damage to various aspects of the environment has further deepened. Therefore, it has become a top priority to study the characteristics of fly ash, increase the utilization of fly ash, and reduce the accumulation of fly ash. At the same time, economic development means a large amount of infrastructure construction, and the demand for coatings has also increased.

[0004] The current anti-corrosion coating preparation process is complex, the filler is single, and the performance of the obtained coating is low. Therefore, it is necessary to make improvements. Summary of the invention

[0005] The present application provides a process for preparing an anti-corrosion coating with added fly ash to solve the problems of high coating preparation cost and environmental pollution, thereby reducing environmental pollution and coating costs, and having dual benefits in both economic and social aspects.

[0006] The present application provides a process for preparing an anti-corrosion coating by adding fly ash, and the process for preparing the anti-corrosion coating comprises the following steps:

[0007] A. Preparation of nano-silicon dioxide;

[0008] B. Modification of nano-silica;

[0009] C. Preparation and modification of nano-silicon dioxide using composite silicon sources in different proportions;

[0010] D. Preparation of nano-silica / epoxy acrylate composite coating;

[0011] E. Testing and characterization of nano-dioxide colloids.

[0012] Preferably, the step A specifically comprises: Based on the method, tetraethyl orthosilicate (TEOS) and deionized water were used as raw materials, ammonia water was used as an alkaline catalyst, and the orthogonal test method was used to determine the preparation of nano-silicon dioxide.

[0013] Preferably, the step B is specifically as follows: preparing nano-silica based on the optimal experimental conditions, and modifying it in situ using a silane coupling agent (γ-aminopropyltriethoxysilane, KH-550), washing the resulting solution three times with anhydrous ethanol by centrifugation, and drying the precipitate obtained by centrifugation in an oven to obtain modified nano-silica solid particles.

[0014] Preferably, the step C specifically includes: selecting TEOS and TMOS in different molar ratios as composite silicon sources, and preparing and modifying nano-silicon dioxide according to optimal experimental conditions.

[0015] Preferably, the step D is specifically as follows: weigh an appropriate amount of deionized water into a coating tank, add a certain amount of dispersant and defoamer in sequence, and then stir and disperse at 500r / min for 10min, then add an appropriate amount of film-forming aids propylene glycol and DMEA in sequence, weigh an appropriate amount of precipitated barium sulfate and titanium dioxide, weigh 2wt% of the epoxy acrylate emulsion mass prepared and modified nano-silicon dioxide from a composite silicon source and add them to the coating tank, respectively recorded as S-1, S-2, S-3, and S-4, and increase the stirring and dispersion rate appropriately, stir and disperse for 20min, and grind with a conical grinder to a fineness of ≤30μm; add an appropriate amount of homemade epoxy acrylate emulsion into the coating tank, stir and disperse, add a certain amount of 420 leveling agent and film-forming aid while stirring and dispersing, disperse for 20min, then add 820 thickener and 810 thickener and disperse for 15min, so as to obtain a one-component water-based epoxy acrylate emulsion composite coating.

[0016] Preferably, the step E specifically comprises: characterizing the basic mechanical properties of the nano-silica coating by measuring conversion rate, adhesion, impact resistance, and hardness indexes; characterizing the anti-corrosion performance of the nano-silica coating by salt spray resistance test and electrochemical test; and structurally characterizing the silica particles by particle size analysis, infrared spectrum analysis, and X-ray diffraction pattern analysis.

[0017] Preferably, the preparation method of the epoxy acrylic emulsion in step D is as follows:

[0018] A. Preparation and characterization of epoxy acrylate soap-free core-shell emulsion:

[0019] Purify acrylic acid and butyl acrylate by a vacuum distillation device, weigh a certain amount of epoxy resin and disperse it in an appropriate amount of butyl acrylate, add it into a four-necked flask, and add an appropriate amount of hydroquinone thereto; in an oil bath at a certain temperature and stir, weigh and mix a certain amount of acrylic acid and triethylamine in a constant pressure dropping funnel, adjust the dropping rate so that it slowly drips into the flask for about 0.5 hours, and keep warm for 3 hours after the dropping is completed to prepare epoxy acrylate;

[0020] B. Synthesis of epoxy acrylate soap-free core-shell emulsion, comprising the following steps:

[0021] The first step is pre-emulsification of the core monomer-epoxy acrylate and the shell monomer-styrene; take two 500mL three-necked flasks, add an appropriate amount of water-dispersed emulsifier aqueous solution, and drop epoxy acrylate and styrene respectively under mechanical stirring. After the slow dropwise addition is completed, adjust the speed to 800r / min and stir for 1h to complete the pre-emulsification process of the core and shell monomers in the two flasks;

[0022] In the second step, the pre-emulsified epoxy acrylate core monomer is transferred to a 250mL four-necked flask, and a proper amount of acrylamide crosslinker and acrylic acid functional monomer are added at a stirring rate of 250r / min, and nitrogen is introduced. While controlling the temperature, the nitrogen introduction time is ensured to be not less than 0.5h; then, the sodium bisulfite-ammonium persulfate initiator is dissolved in water and added to the four-necked flask, and the styrene shell pre-emulsified monomer is added dropwise. After the addition is completed, the temperature is kept for 2h, and the material is discharged after cooling;

[0023] C. Epoxy acrylate soap-free core-shell emulsion film formation:

[0024] The homemade epoxy acrylate soap-free core-shell emulsion and the commercially available ordinary styrene acrylic emulsion were respectively poured into a mold made of polytetrafluoroethylene, the mold having a groove with a length and width of 100 mm and a depth of 1 mm. The mold was placed at room temperature for 24 hours while eliminating bubbles, and then placed in an oven at 80°C for 4 hours. After drying, the film formed by the emulsion was peeled off and placed in a desiccator.

[0025] D. Test the esterification rate, solid content, monomer conversion rate of epoxy acrylate, as well as the gel rate, appearance, mechanical stability, liquid chemical resistance, electrolyte resistance and basic performance of the emulsion; perform infrared spectroscopy, transmission electron microscopy, 13C nuclear magnetic resonance spectroscopy and atomic force microscopy on epoxy acrylate and epoxy acrylate soap-free core-shell emulsion to determine the best experimental conditions for the polymerization process.

[0026] Beneficial effects: Compared with traditional paint fillers, fly ash has similar chemical composition, suitable density, good dispersibility, and certain fluidity, and is gradually used in the paint industry. Fly ash can be reused as a secondary resource to reduce the cost of paint. Since fly ash has particle morphology effect, micro-aggregate effect and volcanic ash activity, fly ash can be used as a filler in various types of paint. The present invention organically combines the high added value utilization of fly ash with the task of energy conservation and emission reduction, which not only increases the comprehensive utilization of fly ash, but also reduces environmental pollution and reduces the cost of paint. It has dual benefits in both economic and social aspects.

[0027] The above description is only an overview of the technical solution of the embodiment of the present application. In order to more clearly understand the technical means of the embodiment of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the embodiments of the present application, a brief introduction will be given below to the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0029] Figure 1 A flow chart is prepared for the present invention;

[0030] Figure 2 This is a schematic diagram of a core or shell monomer pre-emulsification device of the present invention;

[0031] Figure 3 This is a schematic diagram of the epoxy acrylate core-shell emulsion polymerization device of the present invention;

[0032] Figure 4 This is a schematic diagram of a nano-silicon dioxide preparation device of the present invention;

[0033] Figure 5 This is a schematic diagram of the nano-silicon dioxide modification device of the present invention;

[0034] Figure 6 It is a schematic diagram of the vacuum distillation apparatus of the present invention;

[0035] Figure 7 It is a schematic diagram of the epoxy acrylate synthesis device of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used in the specification of the application are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification, claims and drawings of this application are intended to cover non-exclusive inclusions.

[0038] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase "embodiments" in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0039] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the accompanying drawings.

[0040] See also Figure 1-Figure 7 , a process for preparing an anti-corrosion coating by adding fly ash, the process for preparing the anti-corrosion coating comprising the following steps:

[0041] A. Preparation of nano-silicon dioxide;

[0042] B. Modification of nano-silica;

[0043] C. Preparation and modification of nano-silicon dioxide using composite silicon sources in different proportions;

[0044] D. Preparation of nano-silica / epoxy acrylate composite coating;

[0045] E. Testing and characterization of nano-dioxide colloids.

[0046] In the present invention, step A specifically comprises: Based on the method, tetraethyl orthosilicate (TEOS) and deionized water were used as raw materials, ammonia water was used as an alkaline catalyst, and the orthogonal test method was used to determine the preparation of nano-silicon dioxide.

[0047] In the present invention, step B is specifically as follows: preparing nano-silica based on the optimal experimental conditions, and using a silane coupling agent (γ-aminopropyltriethoxysilane, KH-550) to modify it in situ, washing the obtained solution three times with anhydrous ethanol by centrifugation, and placing the precipitate obtained by centrifugation in an oven to dry, thereby obtaining modified nano-silica solid particles.

[0048] In the present invention, step C specifically comprises: selecting TEOS and TMOS in different molar ratios as composite silicon sources, preparing and modifying nano-silicon dioxide according to optimal experimental conditions, wherein the molar ratios of TEOS and TMOS are 3:1, 2:1, 1:1 and 1:2 respectively.

[0049] In the present invention, step D is specifically as follows: weighing an appropriate amount of deionized water into a coating tank, adding a certain amount of dispersant and defoamer in sequence, stirring and dispersing at 500r / min for 10min, then adding an appropriate amount of film-forming aids propylene glycol and DMEA in sequence, weighing an appropriate amount of precipitated barium sulfate and titanium dioxide, weighing 2wt% of the epoxy acrylate emulsion mass prepared and modified nano silicon dioxide from a composite silicon source, adding them to the coating tank, respectively recorded as S-1, S-2, S-3, and S-4, and increasing the stirring and dispersing rate in an appropriate amount, stirring and dispersing for 20min, and grinding the fineness to ≤30μm with a conical grinder; adding an appropriate amount of homemade epoxy acrylate emulsion into the coating tank, stirring and dispersing, adding a certain amount of 420 leveling agent and film-forming aid, dispersing for 20min, and then adding 820 thickener and 810 thickener and dispersing for 15min, so as to obtain a single-component water-based epoxy acrylate emulsion composite coating.

[0050] In the present invention, step E specifically comprises: characterizing the basic mechanical properties of the nano-silicon dioxide coating by measuring conversion rate, adhesion, impact resistance and hardness index; characterizing the anti-corrosion performance of the nano-silicon dioxide coating by salt spray resistance test and electrochemical test; and characterizing the structure of the silicon dioxide particles by particle size analysis, infrared spectrum analysis and X-ray diffraction pattern analysis.

[0051] In the present invention, the preparation method of the epoxy acrylic emulsion in step D is as follows:

[0052] A. Preparation and characterization of epoxy acrylate soap-free core-shell emulsion:

[0053] Purify acrylic acid and butyl acrylate by a vacuum distillation device, weigh a certain amount of epoxy resin and disperse it in an appropriate amount of butyl acrylate, add it into a four-necked flask, and add an appropriate amount of hydroquinone thereto; in an oil bath at a certain temperature and stir, weigh and mix a certain amount of acrylic acid and triethylamine in a constant pressure dropping funnel, adjust the dropping rate so that it slowly drips into the flask for about 0.5 hours, and keep warm for 3 hours after the dropping is completed to prepare epoxy acrylate;

[0054] B. Synthesis of epoxy acrylate soap-free core-shell emulsion, comprising the following steps:

[0055] The first step is pre-emulsification of the core monomer-epoxy acrylate and the shell monomer-styrene; take two 500mL three-necked flasks, add an appropriate amount of water-dispersed emulsifier aqueous solution, and drop epoxy acrylate and styrene respectively under mechanical stirring. After the slow dropwise addition is completed, adjust the speed to 800r / min and stir for 1h to complete the pre-emulsification process of the core and shell monomers in the two flasks;

[0056] In the second step, the pre-emulsified epoxy acrylate core monomer is transferred to a 250mL four-necked flask, and a proper amount of acrylamide crosslinker and acrylic acid functional monomer are added at a stirring rate of 250r / min, and nitrogen is introduced. While controlling the temperature, the nitrogen introduction time is ensured to be not less than 0.5h; then, the sodium bisulfite-ammonium persulfate initiator is dissolved in water and added to the four-necked flask, and the styrene shell pre-emulsified monomer is added dropwise. After the addition is completed, the temperature is kept for 2h, and the material is discharged after cooling;

[0057] C. Epoxy acrylate soap-free core-shell emulsion film formation:

[0058] The homemade epoxy acrylate soap-free core-shell emulsion and the commercially available ordinary styrene acrylic emulsion were respectively poured into a mold made of polytetrafluoroethylene, the mold having a groove with a length and width of 100 mm and a depth of 1 mm. The mold was placed at room temperature for 24 hours while eliminating bubbles, and then placed in an oven at 80°C for 4 hours. After drying, the film formed by the emulsion was peeled off and placed in a desiccator.

[0059] D. Test the esterification rate, solid content, monomer conversion rate of epoxy acrylate, as well as the gel rate, appearance, mechanical stability, liquid chemical resistance, electrolyte resistance and basic performance of the emulsion; perform infrared spectroscopy, transmission electron microscopy, 13C nuclear magnetic resonance spectroscopy and atomic force microscopy on epoxy acrylate and epoxy acrylate soap-free core-shell emulsion to determine the best experimental conditions for the polymerization process.

[0060] In the present invention, the research results of the optimal process for preparing epoxy acrylate soap-free core-shell emulsion and nano-silica particles are used to demonstrate the application of the preparation process optimization technology for preparing new building coatings, and a demonstration production line with an annual output of 200 tons for preparing new nano-inorganic anti-corrosion coatings using industrial solid waste fly ash is built, in order to expand the utilization of solid fly ash waste and achieve the purpose of protecting the environment.

[0061] The present invention selects polymerizable monomer butyl acrylate as the dispersing medium of epoxy resin to prepare epoxy acrylate, uses it as a core monomer after pre-emulsification, uses pre-emulsified styrene as a shell monomer, and adopts a semi-continuous seed emulsion polymerization method to prepare epoxy acrylate soap-free core-shell emulsion under a redox initiation system. By examining the solid content and monomer conversion rate of the emulsion, combined with infrared (FT-IR), transmission electron microscopy (TEM), nuclear magnetic resonance 13C spectrum and other characterization methods, the emulsion is tested and characterized to determine the optimal experimental conditions for the polymerization process.

[0062] In addition, in the present invention, the conversion rate of nano-silica and the particle size of nano-silica microspheres are investigated, and orthogonal experiments are designed to explore the optimal experimental conditions for preparing nano-silica. The structure of nano-silica is characterized by means of FT-IR, XRD and SEM. Under the optimal conditions, different proportions of methyl orthosilicate (TMOS) and ethyl orthosilicate (TEOS) are selected to prepare modified nano-silica, and a homemade epoxy acrylate soap-free core-shell emulsion is selected as a coating film-forming material to prepare a nano-silica / epoxy acrylate composite coating.

[0063] Example:

[0064] The performance test of the anticorrosive coating prepared by the present invention was carried out, and the technical indicators obtained were as follows:

[0065] (1) The surface drying time is 150 minutes, which is better than the surface drying time ≤240 minutes required in the standard (HG / T4759-2014); the actual drying time is 12 hours, which is better than the actual drying time ≤24 hours required in the standard (HG / T4759-2014), solving the problem of long drying time of water-based paints on the market.

[0066] (2) Neutral salt spray resistance is 500h without blistering or shedding, which is better than the 300h required in the standard (HG / T4759-2014).

[0067] (3) Water resistance: no blistering, peeling or rusting for 450 hours, which is better than the 240 hours required in the index (HG / T4759-2014).

[0068] At the same time, the fine processing and deep processing of industrial solid waste fly ash can not only save a lot of resources, but also improve the surrounding environmental pollution. It can not only bring good economic benefits to the enterprise, but also have social benefits of energy saving and environmental protection.

[0069] In summary, compared with traditional paint fillers, fly ash has similar chemical composition, suitable density, good dispersibility, and certain fluidity, and is gradually used in the paint industry. Fly ash can be reused as a secondary resource to reduce the cost of paint. Since fly ash has particle morphology effect, micro-aggregate effect and volcanic ash activity, fly ash can be used as a filler in various types of paint. The present invention organically combines the high added value utilization of fly ash with the task of energy conservation and emission reduction, which not only increases the comprehensive utilization of fly ash, but also reduces environmental pollution and reduces the cost of paint. It has dual benefits in both economic and social aspects.

[0070] As described above, the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A process for preparing an anticorrosive coating with fly ash added, characterized in that: The anti-corrosion coating preparation process includes the following steps: A. Preparation of nano-silicon dioxide; B. Modification of nano-silica; C. Preparation and modification of nano-silicon dioxide using composite silicon sources in different proportions; D. Preparation of nano-silica / epoxy acrylate composite coating; E. Testing and characterization of nano-dioxide colloids.

2. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The step A specifically comprises: Based on the method, tetraethyl orthosilicate (TEOS) and deionized water were used as raw materials, ammonia water was used as an alkaline catalyst, and the orthogonal test method was used to determine the preparation of nano-silicon dioxide.

3. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The step B specifically comprises: preparing nano-silica based on the optimal experimental conditions, and modifying it in situ using a silane coupling agent (γ-aminopropyltriethoxysilane, KH-550), washing the obtained solution three times by centrifugation with anhydrous ethanol, and drying the precipitate obtained by centrifugation in an oven to obtain modified nano-silica solid particles.

4. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The step C specifically includes: selecting TEOS and TMOS with different molar ratios as composite silicon sources, and preparing and modifying nano-silicon dioxide according to optimal experimental conditions.

5. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The step D is specifically as follows: weighing an appropriate amount of deionized water into a coating tank, adding a certain amount of dispersant and defoamer in sequence, and then stirring and dispersing at 500r / min for 10 minutes, then adding an appropriate amount of film-forming aids propylene glycol and DMEA in sequence, weighing an appropriate amount of precipitated barium sulfate and titanium dioxide, weighing 2wt% of the epoxy acrylate emulsion mass prepared and modified nano silicon dioxide from a composite silicon source, and adding them to the coating tank, respectively recorded as S-1, S-2, S-3, and S-4, and increasing the stirring and dispersing rate in an appropriate amount, stirring and dispersing for 20 minutes, and grinding the fineness to ≤30μm with a conical grinder; adding an appropriate amount of homemade epoxy acrylate emulsion into the coating tank, stirring and dispersing, adding a certain amount of 420 leveling agent and film-forming aid, dispersing for 20 minutes, and then adding 820 thickener and 810 thickener and dispersing for 15 minutes, so as to obtain a single-component water-based epoxy acrylate emulsion composite coating.

6. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The step E specifically includes: characterizing the basic mechanical properties of the nano-silicon dioxide coating by measuring conversion rate, adhesion, impact resistance, and hardness indexes; characterizing the anti-corrosion performance of the nano-silicon dioxide coating by salt spray resistance test and electrochemical test; and characterizing the structure of the silicon dioxide particles by particle size analysis, infrared spectrum analysis, and X-ray diffraction pattern analysis.

7. The process for preparing an anticorrosive coating with fly ash added according to claim 1, characterized in that: The preparation method of the epoxy acrylic emulsion in step D is as follows: A. Preparation and characterization of epoxy acrylate soap-free core-shell emulsion: Purify acrylic acid and butyl acrylate by a vacuum distillation device, weigh a certain amount of epoxy resin and disperse it in an appropriate amount of butyl acrylate, add it into a four-necked flask, and add an appropriate amount of hydroquinone thereto; in an oil bath at a certain temperature and stir, weigh and mix a certain amount of acrylic acid and triethylamine in a constant pressure dropping funnel, adjust the dropping rate so that it slowly drips into the flask for about 0.5 hours, and keep warm for 3 hours after the dropping is completed to prepare epoxy acrylate; B. Synthesis of epoxy acrylate soap-free core-shell emulsion, comprising the following steps: The first step is pre-emulsification of the core monomer-epoxy acrylate and the shell monomer-styrene; take two 500mL three-necked flasks, add an appropriate amount of water-dispersed emulsifier aqueous solution, and drop epoxy acrylate and styrene respectively under mechanical stirring. After the slow dropwise addition is completed, adjust the speed to 800r / min and stir for 1h to complete the pre-emulsification process of the core and shell monomers in the two flasks; In the second step, the pre-emulsified epoxy acrylate core monomer is transferred to a 250mL four-necked flask, and a proper amount of acrylamide crosslinker and acrylic acid functional monomer are added at a stirring rate of 250r / min, and nitrogen is introduced. While controlling the temperature, the nitrogen introduction time is ensured to be not less than 0.5h; then, the sodium bisulfite-ammonium persulfate initiator is dissolved in water and added to the four-necked flask, and the styrene shell pre-emulsified monomer is added dropwise. After the addition is completed, the temperature is kept for 2h, and the material is discharged after cooling; C. Epoxy acrylate soap-free core-shell emulsion film formation: The homemade epoxy acrylate soap-free core-shell emulsion and the commercially available ordinary styrene acrylic emulsion were respectively poured into a mold made of polytetrafluoroethylene, the mold having a groove with a length and width of 100 mm and a depth of 1 mm. The mold was placed at room temperature for 24 hours while eliminating bubbles, and then placed in an oven at 80°C for 4 hours. After drying, the film formed by the emulsion was peeled off and placed in a desiccator. D. Test the esterification rate, solid content, monomer conversion rate of epoxy acrylate, as well as the gel rate, appearance, mechanical stability, liquid chemical resistance, electrolyte resistance and basic performance of the emulsion; perform infrared spectroscopy, transmission electron microscopy, 13C nuclear magnetic resonance spectroscopy and atomic force microscopy on epoxy acrylate and epoxy acrylate soap-free core-shell emulsion to determine the best experimental conditions for the polymerization process.