Release agent with low climbing and high residue, preparation method thereof and release film

By using diol hydroxyl double-terminated silicone oil and isocyanatoacrylate and other raw materials to prepare a low-climb high residual release agent, the existing release film in the electronics industry has solved the problems of high VOC and local poor release, and achieved low Climb, high residual effect and good weather resistance and environmental performance.

CN118755407APending Publication Date: 2024-10-11JIANGSU SIDIKE NEW MATERIALS SCI & TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411032928.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing release films used in the electronics industry have problems such as high VOC, high energy consumption, thermal curing environment and poor local release, and it is difficult to achieve low creep and high residual effects.

Method used

Use raw materials such as di-alcohol hydroxyl double-terminated silicone oil and isocyanoacrylate to prepare a low-climb high residual release agent, and form a uniform and dense release coating through UV curing. Combined with photoinitiators and catalysts, stable cross-linking is formed. network to improve adhesion and peel strength.

Benefits of technology

It achieves a low-climb, high-residue release film with good weather resistance and environmental protection performance, avoids the migration of silicone end chains, and maintains a stable peeling effect and low aging climb.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004970380940000101
    Figure BDA0004970380940000101
Patent Text Reader

Abstract

The invention discloses a low-climbing and high-residue release agent, a preparation method thereof and a release liner, the release agent comprises the following raw material components by weight: 5-20 parts of diol hydroxyl double-terminated silicone oil, 1-6 parts of an active diluent, 20-80 parts of isocyano acrylate, 0.025-1 part of p-benzoquinone, 0.01-0.04 part of a catalyst, 15-60 parts of a solvent, and 0.1-0.5 part of a catalyst. 0.75 to 3 parts of 3, 4-ethylenedioxythiophene and 0.25 to 1 part of a photoinitiator. The prepared organic silicon release film has the characteristics of low climbing and high residue, the release coating is uniform and stable, the weather resistance is good, meanwhile, the organic silicon release film is more environment-friendly, and a stable stripping effect on an adhesive tape is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of release materials, and in particular to a release agent with low creep height and residual, a preparation method thereof and a release film. Background Art

[0002] Release films are often used as protective isolation films for pressure-sensitive tapes. They provide ideal peeling force without losing the stickiness of the pressure-sensitive adhesive. This is because silicone resin provides lower surface tension, and substances with higher surface energy are difficult to adhere to. Release films are widely used in daily life and the electronics industry. However, the mainstream release films on the market are basically processed by thermal curing, which leads to high VOC and high energy consumption. The high-temperature curing environment further limits its application in the electronics industry. At the same time, release films often have the defect of poor local release in electronic die-cutting applications. When the machine automatically unwinds, some die slices cannot be separated from the release film, which seriously affects production efficiency and quality. Therefore, it is of great significance to design a new type of high-performance light-curing silicone release agent, which should have uniform and stable surface properties and maintain a high residual adhesion rate under the condition of low release force.

[0003] Patent CN118006248A discloses a release film for silicone OCA and its preparation method, which improves the adhesion between the silicone oil and the substrate by adding a flexible coating between the rigid silicone oil coating and the substrate, thus saving the cost of the protective film. However, this solution uses thermal curing, the production process has high VOC, and it cannot guarantee low residual creep height.

[0004] Patent CN115124749B discloses an antistatic optical release film for OCA optical adhesive and its preparation method, which has a dual antistatic effect by providing an antistatic layer and an antistatic release layer with conductive particles. However, conductive particles are easy to agglomerate, which will lead to poor adhesion of the release layer and a very low residual adhesion rate.

[0005] Therefore, it is necessary to improve the existing technology to provide a more reliable solution. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a release agent with low creep height and residual, a preparation method thereof and a release film in view of the deficiencies in the above-mentioned prior art.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: in the first aspect of the present invention, a release agent with low creep height and residual is provided, comprising the following raw material components in parts by weight:

[0008] 5-20 parts of diol hydroxyl double-terminated silicone oil, 1-6 parts of active diluent, 20-80 parts of isocyanoacrylate, 0.025-1 parts of p-benzoquinone, 0.01-0.04 parts of catalyst, 15-60 parts of solvent, 0.75-3 parts of 3,4-ethylenedioxythiophene, and 0.25-1 parts of photoinitiator.

[0009] Preferably, the isocyanoacrylate is one or more of isocyanoethyl methacrylate, 2-(2-isocyanatoethoxy)ethyl methacrylate and 1,1-bis(acryloyloxymethyl)ethyl isocyanate.

[0010] Preferably, the reactive diluent is dipropylene glycol diacrylate.

[0011] Preferably, the catalyst is dibutyltin dilaurate.

[0012] Preferably, the photoinitiator is hydroxyphenylacetone.

[0013] Preferably, the release agent with low climbing height and high residual comprises the following raw material components in parts by weight:

[0014] 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of isocyanoethyl methyl benzoate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0015] Preferably, the release agent with low climbing height and high residual comprises the following raw material components in parts by weight:

[0016] 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 2-(2-isocyanateethoxy)ethyl methacrylate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0017] Preferably, the release agent with low climbing height and high residual comprises the following raw material components in parts by weight:

[0018] 10 parts of diol hydroxyl di-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 1,1-bis(acryloyloxymethyl)ethyl isocyanate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0019] The second aspect of the present invention provides a method for preparing the release agent with low creep height residue as described above, comprising the following steps:

[0020] S1. Place diol hydroxyl double-terminated silicone oil in a reaction container, heat it to 60-70°C, then add p-benzoquinone, isocyanoacrylate and dibutyltin dilaurate in sequence, stir to react, and use IR to monitor the change of the characteristic peak of -NCO functional group in the system. When the characteristic peak disappears from the spectrum, the reaction is considered to be over, and the reaction is stopped to obtain a release agent;

[0021] S2. Add the obtained release agent to a solvent, then add 3,4-ethylenedioxythiophene, an active diluent, and a photoinitiator, and stir evenly to obtain the release agent with low climb-up and high residual.

[0022] A third aspect of the present invention provides a release film with low creep height residue, which is prepared by the following method:

[0023] The release agent with low climbing height and residual as described above is uniformly coated on the base film, and after UV curing, a release film is obtained.

[0024] The beneficial effects of the present invention are:

[0025] The organic silicon release film prepared by the present invention has low climbing height residual characteristics, the release coating is uniform and stable, and has good weather resistance. It is more environmentally friendly and has a stable peeling effect on the adhesive tape.

[0026] The present invention adopts hydroxypropyl methyl silicone oil with different end-blocking modes to synthesize organosilicon-modified polyurethane (release main agent). When multiple molecules are double-end-blocked, the degree of microphase separation between polar and non-polar groups is small. Under UV curing conditions, there is a strong chemical bond between the organosilicon end chain and the diisocyanate to form a uniform and dense release coating. The diisocyanate is anchored on the substrate, and the migration of the organosilicon end chain to the pressure-sensitive adhesive surface is avoided, thereby ensuring good adhesion and residual bonding.

[0027] Unlike the common alcohol hydroxyl double-terminated silicone oil on the market, the diol hydroxyl double-terminated silicone oil used in the present invention can form a more stable cross-linked network, inhibit the migration of silicone to the pressure-sensitive adhesive, and maintain the peel strength. However, under an aging environment, the cross-linked structure cannot inhibit the migration of polar groups to the surface, so theoretically there will be a higher aging climb; but the measured climb data of the present invention is not high. Through analysis, it is attributed to the fact that in the formula of the present invention, the two free radicals of the dihydroxybutyl double-terminated silicone oil are closer in space, and they are agglomerated and solidified with methylbenzene isocyanate to form a star-shaped structure, which wraps the polar groups. Even under aging conditions, it is difficult for the polar groups to migrate to the surface, resulting in the phenomenon that the release force will not increase rapidly. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with embodiments so that those skilled in the art can implement the invention with reference to the description.

[0029] It should be understood that the terms such as “having”, “including” and “comprising” used herein do not exclude the existence or addition of one or more other elements or combinations thereof.

[0030] The test methods used in the following examples are conventional methods unless otherwise specified. The materials and reagents used in the following examples are all commercially available unless otherwise specified. In the following examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturer is not specified, are all conventional products that can be purchased commercially.

[0031] The present invention provides a release agent with low creep height and residual, comprising the following raw material components in parts by weight:

[0032] 5-20 parts of diol hydroxyl double-terminated silicone oil, 1-6 parts of active diluent, 20-80 parts of isocyanoacrylate, 0.025-1 parts of p-benzoquinone, 0.01-0.04 parts of catalyst, 15-60 parts of solvent, 0.75-3 parts of 3,4-ethylenedioxythiophene, and 0.25-1 parts of photoinitiator.

[0033] In a preferred embodiment, the isocyanoacrylate is a highly reactive isocyano(meth)acrylate capping agent, specifically one or more of isocyanoethyl methacrylate, 2-(2-isocyanatoethoxy)ethyl methacrylate and 1,1-bis(acryloyloxymethyl)ethyl isocyanate.

[0034] In a preferred embodiment, the reactive diluent is dipropylene glycol diacrylate.

[0035] In a preferred embodiment, the catalyst is dibutyltin dilaurate.

[0036] In a preferred embodiment, the photoinitiator is hydroxyphenylacetone.

[0037] In a preferred embodiment, the low-climbing residual release agent comprises the following raw material components in parts by weight:

[0038] 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of isocyanoethyl methyl benzoate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0039] In a preferred embodiment, the low-climbing residual release agent comprises the following raw material components in parts by weight:

[0040] 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 2-(2-isocyanateethoxy)ethyl methacrylate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0041] In a preferred embodiment, the low-climbing residual release agent comprises the following raw material components in parts by weight:

[0042] 10 parts of diol hydroxyl di-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 1,1-bis(acryloyloxymethyl)ethyl isocyanate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

[0043] The present invention also provides a method for preparing the above-mentioned release agent with low climbing height and high residual, comprising the following steps:

[0044] S1. Place diol hydroxyl double-terminated silicone oil in a reaction container, heat it to 60-70°C, then add p-benzoquinone, isocyanoacrylate and dibutyltin dilaurate in sequence, stir to react, and use IR to monitor the change of the characteristic peak of -NCO functional group in the system. When the characteristic peak disappears from the spectrum, the reaction is considered to be over, and the reaction is stopped to obtain a release agent;

[0045] S2. Add the obtained release agent to the solvent, then add 3,4-ethylenedioxythiophene and active diluent to inhibit the self-polymerization of the release agent in a hot environment, then add a photoinitiator, stir evenly, and obtain a release agent with low climbing height and high residual.

[0046] The present invention also provides a release film with low creep height and low residual, characterized in that it is prepared by the following method:

[0047] The above-mentioned low-climbing residual release agent is evenly coated on the base film, and after UV curing, a release film is obtained.

[0048] The above is the overall concept of the present invention, and detailed embodiments and comparative examples are provided below on the basis of the overall concept of the present invention to further illustrate the present invention.

[0049] The sources of the main raw materials involved in the following examples and comparative examples are described as follows:

[0050] Diol hydroxyl double-terminated silicone oil Wuhan Lanabai Pharmaceutical Chemical Co., Ltd. INB-1233;

[0051] Alcohol hydroxyl double-terminated silicone oil Anhui Mingyi Silicon Industry Co., Ltd. MY-8815;

[0052] Bis(ol)hydroxyl mono-terminated silicone oil Anhui IOTA Silicone Oil Co., Ltd. IOTA8866;

[0053] Isocyanoethyl methyl benzoate Nanjing Kangmanlin Biopharmaceutical Technology Co., Ltd.;

[0054] 2-(2-isocyanatoethoxy)ethyl methacrylate Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;

[0055] 1,1-Bis(acryloyloxymethyl)ethyl isocyanate Wuhan Huaxiang Kejie Biotechnology Co., Ltd.;

[0056] p-Benzoquinone Aladdin Biochemical Technology Co., Ltd.;

[0057] Dibutyltin dilaurate Aladdin Biochemical Technology Co., Ltd.;

[0058] 3,4-ethylenedioxythiophene Hubei Xingyan New Material Technology Co., Ltd.;

[0059] Dipropylene glycol diacrylate Jiangsu Runfeng Synthetic Technology Co., Ltd.;

[0060] Hydroxyphenylacetone Jiangsu Guangxin Photosensitive New Materials Co., Ltd.

[0061] Example 1

[0062] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0063] S1. Weigh 10g of diol hydroxyl double-terminated silicone oil and place it in a reactor. After the system temperature rises to 65°C, add 0.05g of p-benzoquinone, 40g of methylbenzoic acid isocyanoethyl ester and 0.02g of dibutyltin dilaurate to the reactor in sequence; continue to stir at high speed (stirring speed is 500 rpm), use IR to monitor the change of the characteristic peak of the -NCO functional group in the system, and when the characteristic peak disappears from the spectrum, the reaction is considered to be completed, and finally a stable yellow product is formed to obtain a release agent;

[0064] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 10%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent dipropylene glycol diacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0065] A release film with low climbing height residue is prepared by the following method:

[0066] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing. The UV lamp power was 80% and the oxygen content was below 5PPM. For a release film with a thickness of 500nm, the above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0067] Example 2

[0068] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0069] S1. Weigh 10g of diol hydroxyl double-terminated silicone oil and place it in a reactor. After the system temperature rises to 65°C, add 0.05g of p-benzoquinone, 40g of 2-(2-isocyanatoethoxy)ethyl methacrylate and 0.02g of dibutyltin dilaurate to the reactor in sequence; continue to stir at high speed (stirring speed is 500 rpm), use IR to monitor the change of the characteristic peak of the -NCO functional group in the system, and when the characteristic peak disappears from the spectrum, the reaction is considered to be completed, and finally a stable yellow product is formed to obtain a release agent;

[0070] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 10%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent dipropylene glycol diacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0071] A release film with low climbing height residue is prepared by the following method:

[0072] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing. The UV lamp power was 80% and the oxygen content was below 5PPM. A release film with a dry glue thickness of 500nm was obtained. The above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0073] Example 3

[0074] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0075] S1. Weigh 10g of diol hydroxyl double-terminated silicone oil and place it in a reactor. After the system temperature rises to 65°C, add 0.05g of p-benzoquinone, 40g of 1,1-bis(acryloyloxymethyl)ethyl isocyanate acrylate and 0.02g of dibutyltin dilaurate to the reactor in sequence; continue to stir at high speed (stirring speed is 500 rpm), use IR to monitor the change of the characteristic peak of the -NCO functional group in the system, and when the characteristic peak disappears from the spectrum, the reaction is considered to be completed, and finally a stable yellow product is formed to obtain a release agent;

[0076] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 10%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent dipropylene glycol diacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0077] A release film with low climbing height residue is prepared by the following method:

[0078] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing. The UV lamp power was 80% and the oxygen content was below 5PPM. A release film with a dry glue thickness of 500nm was obtained. The above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0079] Comparative Example 1

[0080] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0081] S1. Weigh 10g of diol hydroxyl double-terminated silicone oil and place it in a reactor, add 30g of ethyl acetate and stir evenly, add 1.5g of toluene diisocyanate after the system temperature rises to 65°C, stir at high speed (stirring speed is 500 rpm) for 5h to form a yellow viscous liquid; then add 0.05g of p-benzoquinone to the reactor, stir at high speed (stirring speed is 500 rpm) for 20min, then add 1.5g of pentaerythritol triacrylate and 0.02g of dibutyltin dilaurate in sequence, continue to stir at high speed (stirring speed is 500 rpm) at 65°C system temperature for 2h to finally form a stable yellow product to obtain a release agent;

[0082] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 5%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent pentaerythritol tetraacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0083] A release film with low climbing height residue is prepared by the following method:

[0084] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing. The UV lamp power was 80% and the oxygen content was below 5PPM. A release film with a dry glue thickness of 500nm was obtained. The above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0085] Comparative Example 2

[0086] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0087] S1. Weigh 10g of alcohol hydroxyl double-terminated silicone oil and place it in a reactor. After the system temperature rises to 65°C, add 0.05g of p-benzoquinone, 40g of methylbenzoic acid isocyanoethyl ester and 0.02g of dibutyltin dilaurate to the reactor in sequence; continue to stir at high speed (stirring speed is 500 rpm), use IR to monitor the change of the characteristic peak of the -NCO functional group in the system, and when the characteristic peak disappears from the spectrum, the reaction is considered to be completed, and finally a stable yellow product is formed to obtain a release agent;

[0088] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 5%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent dipropylene glycol diacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0089] A release film with low climbing height residue is prepared by the following method:

[0090] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing with a UV lamp power of 80% and an oxygen content of less than 5PPM. A release film with a dry adhesive thickness of 500nm was obtained. The above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0091] Comparative Example 3

[0092] A release agent with low climbing height and residual, the preparation method of which comprises the following steps:

[0093] S1. Weigh 10g of diol hydroxyl mono-terminated silicone oil and place it in a reactor. After the system temperature rises to 65°C, add 0.05g of p-benzoquinone, 40g of isocyanoethyl methylbenzene and 0.02g of dibutyltin dilaurate to the reactor in sequence; continue to stir at high speed (stirring speed is 500 rpm), use IR to monitor the change of the characteristic peak of the -NCO functional group in the system, and when the characteristic peak disappears from the spectrum, the reaction is considered to be completed, and finally a stable yellow product is formed to obtain a release agent;

[0094] S2. The prepared release agent is diluted with 30g of ethyl acetate to a solid content of 5%, and 1.5g of 3,4-ethylenedioxythiophene and 2g of active diluent dipropylene glycol diacrylate are added to inhibit the self-polymerization of the release agent in a hot environment, and then 0.5g of photoinitiator hydroxyphenylacetone is added, and the mixture is mixed using a magnetic stirrer to obtain a release agent.

[0095] A release film with low climbing height residue is prepared by the following method:

[0096] The prepared release agent was evenly coated on a 50μm PET film using a wire rod. The coated sample was discharged and isolated from the air using a fluorine release film. After standing for 20 minutes, it was placed in a UV light curing machine for curing. The UV lamp power was 80% and the oxygen content was below 5PPM. A release film with a dry glue thickness of 500nm was obtained. The above steps must be completed in a light-proof environment. After standing for 24 hours, the mechanical properties of the release film were tested.

[0097] The release films prepared in Examples 1-3 and Comparative Examples 1-3 were subjected to the following performance tests:

[0098] 1. 20min, 24H test method: Standard tape TESA7475 is attached to the release surface, and rolled back and forth twice with a 2kg roller (300mm / min), then placed at room temperature (23±2℃, relative humidity 50%) for 20min and 24H, and then peeled 180° at 300mm / min with a universal tensile testing machine, tested 3 times, and the average value is recorded as the 20min, 24H release force

[0099] 2. Test method: Standard tape TESA7475 is attached to the release surface, rolled back and forth twice with a 2kg roller (300mm / min), then placed in a 55°C oven, aged for 20 hours, taken out and placed at room temperature for 2 hours, then peeled 180° at 300mm / min using a universal tensile testing machine, tested 3 times, and the average value was taken.

[0100] 4. Residual test method: The standard tape Nitto 31B is attached to the release surface, and rolled back and forth twice with a 2kg roller (300mm / min), then placed in a 55°C oven, aged for 20 hours, taken out and placed at room temperature for 2 hours, the Nitto 31B on the test sample is peeled off and attached to a standard steel plate, and rolled back and forth twice with a 2kg roller. After standing for 20 minutes, the peeling force is tested and recorded as A1. The standard tape Nitto 31B is attached to the release standard steel plate, and rolled back and forth twice with a 2kg roller (300mm / min). After standing for 20 minutes, the peeling force is tested and recorded as A2. Residual SA% = (A1 / A2) × 100%

[0101] 5. Performance evaluation (the evaluation index is the comprehensive performance of residual and aging climb, and the residual is greater than 85% and the residual climb is less than 20g, which is excellent)

[0102] The test results are shown in Table 1 below:

[0103] Table 1

[0104]

[0105] According to the test results in Table 1, it can be seen that the release films of Examples 1-3 have the characteristics of low climb and high residual, which is mainly attributed to the fact that under UV curing conditions, the silicone-modified polyurethane synthesized from diol hydroxyl di-terminated silicone oil and isocyanobenzoic ester can maintain a low aging release force climb while ensuring a high residual under the premise of avoiding the harm of organic solvents to the environment.

[0106] According to the comparison of the results of the embodiment and the comparative example, it can be explained that the silicone-modified polyurethane synthesized from diol hydroxyl diblocked silicone oil and active isocyanobenzoic acid shows higher residual and lower aging climb than the silicone-modified polyurethane with ordinary diol hydroxyl diblocked silicone oil and diol hydroxyl monoblocked silicone oil as reaction substrates.

[0107] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to specific details.

Claims

1. A release agent with low creep height and residual strength. It is characterized in that The invention comprises the following raw material components by weight: 5-20 parts of diol hydroxyl double-terminated silicone oil, 1-6 parts of active diluent, 20-80 parts of isocyanoacrylate, 0.025-1 parts of p-benzoquinone, 0.01-0.04 parts of catalyst, 15-60 parts of solvent, 0.75-3 parts of 3,4-ethylenedioxythiophene, and 0.25-1 parts of photoinitiator.

2. The release agent with low climbing height and high residual according to claim 1, It is characterized in that The isocyanoacrylate is one or more of isocyanoethyl methacrylate, 2-(2-isocyanatoethoxy)ethyl methacrylate and 1,1-bis(acryloyloxymethyl)ethyl isocyanate.

3. The release agent with low creep height and high residual according to claim 1, It is characterized in that The active diluent is dipropylene glycol diacrylate.

4. The release agent with low climbing height and high residual according to claim 1, It is characterized in that The catalyst is dibutyltin dilaurate.

5. The release agent with low creep height and high residual according to claim 1, It is characterized in that The photoinitiator is hydroxyphenylacetone.

6. The release agent with low creep height and residual amount according to claim 1, It is characterized in that The invention comprises the following raw material components by weight: 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of isocyanoethyl methyl benzoate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

7. The release agent with low creep height and residual amount according to claim 1, It is characterized in that The invention comprises the following raw material components by weight: 10 parts of diol hydroxyl double-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 2-(2-isocyanateethoxy)ethyl methacrylate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

8. The release agent with low climbing height and high residual according to claim 1, It is characterized in that The invention comprises the following raw material components by weight: 10 parts of diol hydroxyl di-terminated silicone oil, 2 parts of dipropylene glycol diacrylate, 40 parts of 1,1-bis(acryloyloxymethyl)ethyl isocyanate, 0.05 parts of p-benzoquinone, 0.02 parts of dibutyltin dilaurate, 30 parts of ethyl acetate, 1.5 parts of 3,4-ethylenedioxythiophene, and 0.5 parts of hydroxyphenylacetone.

9. A method for preparing a release agent with low creep height and high residual as claimed in any one of claims 1 to 8, It is characterized in that The following steps are involved: S1. Place diol hydroxyl double-terminated silicone oil in a reaction container, heat it to 60-70°C, then add p-benzoquinone, isocyanoacrylate and dibutyltin dilaurate in sequence, stir to react, and use IR to monitor the change of the characteristic peak of -NCO functional group in the system. When the characteristic peak disappears from the spectrum, the reaction is considered to be over, and the reaction is stopped to obtain a release agent; S2. Add the obtained release agent to a solvent, then add 3,4-ethylenedioxythiophene, an active diluent, and a photoinitiator, and stir evenly to obtain the release agent with low climb-up and high residual.

10. A release film with low climbing height and residual, It is characterized in that It is prepared by the following method: The release agent with low creep height and high residual as claimed in any one of claims 1 to 8 is uniformly coated on the base film, and after UV curing, a release film is obtained.

Citation Information

Cited By

  • Release agent with low release-force increase and high residual adhesion and preparation method therefor, and release film

    WO2026025777A1