Method for improving lubricating performance and cleaning performance of copper wire corrosion-resistant wire drawing liquid

Through the synergistic effect of ester compounds and polyether compounds, combined with specific anti-rust agents and corrosion inhibitors, the lubrication and cleaning properties of the copper wire drawing liquid are optimized, solving the instability problem in the existing technology and achieving higher performance. Lubricity and corrosion resistance extend service life.

CN118755518APending Publication Date: 2024-10-11GUANGZHOU LANDNOK CHEM TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410824437.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-09-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The lubrication and cleaning properties of existing copper wire drawing fluids are unstable, leading to wire shrinkage, wire breakage and mold damage, making it difficult to meet the requirements of high-tech applications.

Method used

Using the synergistic effect of ester compounds and polyether compounds, combined with acyl amino acids, lauric acid, benzotriazole and other ingredients, through specific ratios and process steps, an optimized drawing fluid is formed to improve lubrication and anti-corrosion properties. .

Benefits of technology

It significantly improves the lubrication performance and cleaning ability of the wire drawing fluid, avoids wire shrinkage and wire breakage, ensures the surface brightness and anti-oxidation ability of the wire, and extends the service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004910054380000071
    Figure BDA0004910054380000071
Patent Text Reader

Abstract

The invention provides a method for improving the lubricating performance and the cleaning performance of a copper wire corrosion-resistant wire drawing liquid, and relates to the technical field of metal wire drawing liquid. The method comprises the steps of preparation of the lubricant and preparation of the wire drawing liquid. Through the synergistic effect of triethanolamine oleate, trans-block polyether and acylamino acid, the lubricating property of the wire drawing liquid is improved, acylamino acid and dodecanedioic acid are used as antirust agents, the lubricating property, corrosion resistance and cleaning capacity of the wire drawing liquid are improved, and the wire drawing liquid is suitable for being used in the field of wire drawing. Through a precipitation film formed by metal ions generated in the corrosion process of benzotriazole and copper wires, the corrosion resistance and the cleaning capacity of the wire drawing liquid are improved, fine copper powder is promoted to rapidly settle, it is guaranteed that liquid feeding is stable and free of impurities, and the service life can be prolonged to 6 months or above from 3 months.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal wire drawing liquid, and in particular to a method for improving the lubrication performance and cleaning performance of copper wire corrosion resistant wire drawing liquid. Background Art

[0002] Drawing process is a common metal processing method. Microwires usually refer to fine metal wires with diameters ranging from a few microns to tens of microns, which are usually used in various high-tech and precision applications, such as electronic equipment, sensors, medical equipment, optical equipment, etc. At present, microwires are generally made by drawing process, in which lubrication during the drawing process plays a key role in the preparation of microwires. In the prior art, the lubricant and anti-corrosion agent in the drawing liquid used in copper micromachining will compete to be adsorbed on the surface of the copper wire, resulting in unstable lubrication and cleaning performance, and will also cause certain damage to the mold.

[0003] Patent CN201910925481.X discloses a fully synthetic cutting fluid and a preparation method thereof, including ingredients such as polyether and benzotriazole. The product has a self-defoaming function and a clear appearance, but does not solve the problem of unstable lubrication and cleaning performance.

[0004] Patent CN201710325539.8 discloses a low pH aviation aluminum alloy cutting fluid and its preparation and application, which includes triethanolamine oleate, tall oil, triethanolamine and other ingredients. The corrosion inhibition effect and lubrication performance of the product are improved, but the cleaning performance is not improved.

[0005] Therefore, developing a wire drawing liquid that can simultaneously improve the lubrication performance and cleaning performance of the copper wire drawing liquid is one of the technical problems that urgently need to be solved in this field. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a method for improving the lubrication performance and cleaning performance of copper wire corrosion-resistant drawing liquid, which specifically comprises the following steps:

[0007] S1. Weigh an ester compound and a polyether compound by weight, mix them, and stir them at 80° C. until they become transparent to obtain a lubricant;

[0008] S2, weighing pH regulator and low carbonic acid by weight, adding them into a 10000L electrically heated stainless steel reactor, heating to 110°C, keeping warm for 2h, then cooling to 50°C, and then adding deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and defoaming agent by weight in sequence, stirring for 1h;

[0009] The mass fractions of each component in S2 are as follows:

[0010] Rust inhibitor 3-10 parts, pH adjuster 10-30 parts, lubricant 10-40 parts, low carbonic acid 1-3 parts, corrosion inhibitor 0.1-2 parts, wetting agent 0.1-1.5 parts, defoamer 0-0.3 parts, deionized water 20-80 parts.

[0011] Furthermore, the mass fractions of each component in S2 are as follows:

[0012] Rust inhibitor 6-10 parts, pH adjuster 20-30 parts, lubricant 20-30 parts, low carbonic acid 2-3 parts, corrosion inhibitor 1-2 parts, wetting agent 0.5-1.5 parts, defoamer 0.1-0.3 parts, deionized water 20-80 parts.

[0013] Preferably, the mass fractions of each component in S2 are as follows:

[0014] 8 parts of rust inhibitor, 25 parts of pH adjuster, 25 parts of lubricant, 2 parts of low carbonic acid, 1 part of corrosion inhibitor, 1 part of wetting agent, 0.2 parts of defoaming agent, and 80 parts of deionized water.

[0015] Furthermore, the rust inhibitor is one or more of ternary polycarboxylic acid, sebacic acid, lauric acid, acylamino acid, and sulfonamide acid-type rust inhibitors. Preferably, the rust inhibitor is acylamino acid and lauric acid.

[0016] Furthermore, the rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.5.

[0017] Further, the pH regulator is one or more of monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, and diisopropanolamine. Preferably, the pH regulator is triethanolamine.

[0018] Furthermore, the lubricant is one or both of an ester compound and a polyether compound.

[0019] Furthermore, the lubricant is composed of an ester compound and a polyether compound in a mass ratio of 1:1.

[0020] Further, the HLB value of the polyether compound is less than 9. Preferably, the HLB value of the polyether compound is 7.

[0021] Furthermore, the ester compound is triethanolamine oleate, and the polyether compound is a trans-block polyether.

[0022] Further, the low carbonic acid is one or more of neodecanoic acid, isononanoic acid, and isodecanoic acid. Preferably, the low carbonic acid is neodecanoic acid.

[0023] Furthermore, the corrosion inhibitor is one or more of benzotriazole, methylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-benzotriazole-methyl methacrylate, poly(1-benzotriazole-methyl methacrylate-methyl acrylate) and poly(1-benzotriazole-methyl methacrylate-acrylic acid).

[0024] Furthermore, the corrosion inhibitor is benzotriazole.

[0025] Furthermore, the wetting agent is an acetylenic alcohol surfactant. Preferably, the wetting agent is an acetylenic diol surfactant.

[0026] Furthermore, the defoamer is an organosilicon defoamer. Preferably, the defoamer is a highly compatible silicone polyether defoamer.

[0027] Compared with the prior art, the beneficial technical effects of the present invention are:

[0028] The present invention improves the lubricity of the wire drawing liquid through the synergistic effect of triethanolamine oleate, trans-block polyether and acylamino acid, effectively avoids wire shrinkage and wire breakage caused by poor lubrication stability during the wire drawing process, thereby ensuring stable wire diameter.

[0029] The lubricating performance of the wire drawing liquid of the present invention is significantly improved, thereby enabling the surface of the wire to have high brightness and no color light, and enabling the finished wire to have a good surface state.

[0030] The present invention uses acylamino acid and lauric acid as rust inhibitors, and under the action of triethanolamine, further improves the lubrication performance, corrosion resistance and cleaning ability of the wire drawing liquid, can effectively prevent the adhesion of copper soap and copper powder on the wire drawing die, avoids clogging of the die hole, and can reduce the wire breakage rate and improve the antioxidant capacity of the copper wire to meet the storage requirements between processes.

[0031] The benzotriazole of the present invention can form a precipitation film with the metal ions generated during the corrosion process of the copper wire, further improving the corrosion resistance and cleaning ability of the wire drawing liquid, promoting the rapid sedimentation of fine copper powder, ensuring that the liquid is stable and free of impurities, and the service life can be extended from 3 months to more than 6 months. DETAILED DESCRIPTION

[0032] The present invention provides a method for improving the lubrication performance and cleaning performance of a copper wire corrosion-resistant wire drawing liquid, which specifically comprises the following steps:

[0033] S1. Weigh an ester compound and a polyether compound by weight, mix them, and stir them at 80° C. until they become transparent to obtain a lubricant;

[0034] S2, weighing pH regulator and low carbonic acid by weight, adding them into a 10000L electrically heated stainless steel reactor, heating to 110°C, keeping warm for 2h, then cooling to 50°C, and then adding deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and defoaming agent by weight in sequence, stirring for 1h;

[0035] The mass fractions of each component in S2 are as follows:

[0036] Rust inhibitor 3-10 parts, pH adjuster 10-30 parts, lubricant 10-40 parts, low carbonic acid 1-3 parts, corrosion inhibitor 0.1-2 parts, wetting agent 0.1-1.5 parts, defoamer 0-0.3 parts, deionized water 20-80 parts.

[0037] In one embodiment, the mass fractions of the components in S2 are as follows:

[0038] Rust inhibitor 6-10 parts, pH adjuster 20-30 parts, lubricant 20-30 parts, low carbonic acid 2-3 parts, corrosion inhibitor 1-2 parts, wetting agent 0.5-1.5 parts, defoamer 0.1-0.3 parts, deionized water 20-80 parts.

[0039] In one embodiment, the mass fractions of the components in S2 are as follows:

[0040] 8 parts of rust inhibitor, 25 parts of pH adjuster, 25 parts of lubricant, 2 parts of low carbonic acid, 1 part of corrosion inhibitor, 1 part of wetting agent, 0.2 parts of defoaming agent, and 80 parts of deionized water.

[0041] In one embodiment, the rust inhibitor is one or more of ternary polycarboxylic acid, sebacic acid, lauric acid, acylamino acid, and sulfonamide acid-type rust inhibitors.

[0042] In one embodiment, the rust inhibitor is acylamino acid and lauric acid.

[0043] In one embodiment, the rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.5.

[0044] In the present invention, the carboxylate ammonium salt generated by the reaction of lauric acid and triethanolamine can be adsorbed on the metal surface to improve the corrosion resistance of the wire drawing liquid. At the same time, the acylamino acid can couple with the trans-block polyether to promote the compatibility of the trans-block polyether in the wire drawing liquid, and improve the lubrication performance and corrosion resistance of the wire drawing liquid. Therefore, the present invention preferably uses acylamino acid and lauric acid as rust inhibitors.

[0045] In one embodiment, the pH regulator is one or more of monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, and diisopropanolamine. Preferably, the pH regulator is triethanolamine.

[0046] In one embodiment, the lubricant is one or both of an ester compound and a polyether compound.

[0047] In one embodiment, the lubricant is composed of an ester compound and a polyether compound in a mass ratio of 1:1.

[0048] In one embodiment, the HLB value of the polyether compound is less than 9.

[0049] In one embodiment, the HLB value of the polyether compound is 7.

[0050] In one embodiment, the ester compound is triethanolamine oleate, and the polyether compound is a trans-block polyether.

[0051] In the present invention, the HLB value of the trans-block polyether is too large, the number of polyoxyethylene increases, and the hydrophilicity is too strong, resulting in poor compatibility with ester compounds, thereby affecting the lubrication performance. When the HLB value of the trans-block polyether is less than 9, the compatibility of the trans-block polyether with triethanolamine oleate is enhanced. The reason is that triethanolamine oleate contains ester groups, the HLB value of the trans-block polyether is small, the lipophilicity becomes stronger, and it is easier to react with the ester groups in triethanolamine oleate, thereby promoting the compatibility between the two, so that the trans-block polyether can also maintain good lubricity during processing. At the same time, acyl amino acids can also promote the compatibility of trans-block polyethers. The synergistic effect of the three enables the trans-block polyether to be stably precipitated on the metal surface, ensuring the lubrication effect. Therefore, the present invention strictly limits the said

[0052] In one embodiment, the low carbonic acid is one or more of neodecanoic acid, isononanoic acid, and isodecanoic acid.

[0053] In one embodiment, the oligocarboxylic acid is neodecanoic acid.

[0054] In one embodiment, the corrosion inhibitor is one or more of benzotriazole, methylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-benzotriazole-methyl methacrylate, poly(1-benzotriazole-methyl methacrylate-methyl acrylate) and poly(1-benzotriazole-methyl methacrylate-acrylic acid).

[0055] In one embodiment, the corrosion inhibitor is benzotriazole.

[0056] The corrosion inhibitor in the present invention interacts with metal ions to form a precipitation film to improve the cleaning ability of the product. However, it was found during the research process that excessive use of the corrosion inhibitor would damage the film. Therefore, the present invention strictly limits the amount of the slow-release agent to ensure the effective formation of the precipitation protective film, thereby improving the corrosion resistance and cleaning ability of the wire drawing liquid.

[0057] In one embodiment, the wetting agent is an acetylenic alcohol surfactant.

[0058] In one embodiment, the wetting agent is an acetylenic diol surfactant.

[0059] In one embodiment, the defoaming agent is a silicone defoaming agent.

[0060] In one embodiment, the defoaming agent is a highly compatible silicone polyether defoaming agent.

[0061] The technical solution of the present invention is described in detail below through embodiments, but the protection scope of the present invention is not limited to the embodiments.

[0062] In a specific embodiment of the present invention, the model of the acyl amino acid is NEUF585-2, purchased from Notai Technology; the trans-block polyether, brand L62, purchased from Jiahua Chemical, HLB value is 7, brand L63, HLB value is 11; the acetylene glycol surfactant, model Surfynol485, purchased from Evonik; the defoamer is a highly compatible silicone polyether defoamer, model ZY-2168, purchased from Shanghai Ziyi.

[0063] Example 1

[0064] A method for improving the lubrication and cleaning performance of a copper wire anti-corrosion drawing fluid, comprising the following steps:

[0065] S1. Weigh triethanolamine oleate and trans-block polyether by weight and add them into a 1000L electrically heated stainless steel reactor, mix them, and stir them at 80°C until they become transparent to obtain a lubricant;

[0066] S2, weighing pH regulator and low carbonic acid by weight, adding them into a 10000L electrically heated stainless steel reactor, heating to 110°C, keeping warm for 2 hours, then cooling to 50°C, and then adding deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and highly compatible silicone polyether defoamer by weight in sequence, stirring for 1 hour;

[0067] The S2 comprises, by weight:

[0068] 8 parts of rust inhibitor, 25 parts of triethanolamine, 25 parts of lubricant, 2 parts of neodecanoic acid, 1 part of benzotriazole, 1 part of acetylene glycol surfactant, 0.2 parts of highly compatible silicone polyether defoamer, and 80 parts of deionized water.

[0069] The rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.5.

[0070] The mass ratio of the triethanolamine oleate and the trans-block polyether is 1:1.

[0071] Example 2

[0072] A method for improving the lubrication and cleaning performance of a copper wire anti-corrosion drawing fluid, comprising the following steps:

[0073] S1. Weigh triethanolamine oleate and trans-block polyether by weight and add them into a 1000L electrically heated stainless steel reactor, mix them, and stir them at 80°C until they become transparent to obtain a lubricant;

[0074] S2, weighing pH regulator and low carbonic acid by weight, adding them into a 10000L electrically heated stainless steel reactor, heating to 110°C, keeping warm for 2 hours, then cooling to 50°C, and then adding deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and highly compatible silicone polyether defoamer by weight in sequence, stirring for 1 hour;

[0075] The S2 comprises, by weight:

[0076] 10 parts of rust inhibitor, 30 parts of triethanolamine, 40 parts of lubricant, 3 parts of neodecanoic acid, 2 parts of benzotriazole, 1.5 parts of acetylene glycol surfactant, 0.3 parts of highly compatible silicone polyether defoamer, and 80 parts of deionized water.

[0077] The rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.5.

[0078] The mass ratio of the triethanolamine oleate and the trans-block polyether is 1:1.

[0079] Example 3

[0080] A method for improving the lubrication and cleaning performance of a copper wire anti-corrosion drawing fluid, comprising the following steps:

[0081] S1. Weigh triethanolamine oleate and trans-block polyether by weight and add them into a 1000L electrically heated stainless steel reactor, mix them, and stir them at 80°C until they become transparent to obtain a lubricant;

[0082] S2, weighing pH regulator and low carbonic acid by weight, adding them into a 10000L electrically heated stainless steel reactor, heating to 110°C, keeping warm for 2 hours, then cooling to 50°C, and then adding deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and highly compatible silicone polyether defoamer by weight in sequence, stirring for 1 hour;

[0083] The S2 comprises, by weight:

[0084] 6 parts of rust inhibitor, 20 parts of triethanolamine, 20 parts of neodecanoic acid, 2 parts of benzotriazole, 1 part of corrosion inhibitor, 0.5 parts of acetylene glycol surfactant, 0.1 parts of highly compatible silicone polyether defoamer, and 80 parts of deionized water.

[0085] The rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.5.

[0086] The mass ratio of the triethanolamine oleate and the trans-block polyether is 1:1.

[0087] Comparative Example 1

[0088] Same as Example 1, except that the lubricant is triethanolamine oleate.

[0089] Comparative Example 2

[0090] Same as Example 1, except that: the rust inhibitor is acylamino acid, and the pH adjuster is monoethanolamine.

[0091] Comparative Example 3

[0092] The same as Example 1, except that the rust inhibitor is composed of acylamino acid and lauric acid in a mass ratio of 1:1.

[0093] Comparative Example 4

[0094] Same as Example 1, except that: the rust inhibitor is lauric acid; and the HLB value of the trans-block polyether is 11.

[0095] The performance of the products of Examples 1-3 and Comparative Examples 1-4 was tested as follows:

[0096] 1. The anti-rust and corrosion performance test refers to GB / T6144-2010 test, and the results are shown in Table 1.

[0097] 2. Lubrication performance test: The maximum no-seizure load PB value was determined using the MRS-10A four-ball friction and wear testing machine produced by Jinan Star Testing Technology Co., Ltd.

[0098] Table 1 Product performance test results

[0099]

[0100] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for improving the lubrication and cleaning properties of a copper wire corrosion-resistant drawing fluid, characterized in that: The following steps are involved: S1. Weigh an ester compound and a polyether compound in parts by weight, mix them, and stir them at 80° C. until they become transparent to obtain a lubricant; S2. Weigh the pH regulator and low carbonic acid by weight and add them to a 10,000 L electrically heated stainless steel reactor, heat to 110° C., keep warm for 2 hours, then cool to 50° C., then add deionized water, the lubricant, rust inhibitor, corrosion inhibitor, wetting agent and defoamer by weight in sequence, and stir for 1 hour; The mass fractions of each component in S2 are as follows: 3-10 parts of rust inhibitor, 10-30 parts of pH regulator, 10-40 parts of lubricant, 1-3 parts of low carbonic acid, 0.1-2 parts of corrosion inhibitor, 0.1-1.5 parts of wetting agent, 0-0.3 parts of defoaming agent, 20-80 parts of deionized water.

2. The method for improving the lubrication and cleaning properties of the copper wire corrosion-resistant drawing liquid according to claim 1, characterized in that: The rust preventive agent is one or more of ternary polycarboxylic acid, sebacic acid, lauric acid, acylamino acid, and sulfonamide acid type rust preventive agents.

3. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 1, characterized in that: The pH regulator is one or more of monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, and diisopropanolamine.

4. The method for improving the lubrication and cleaning properties of a copper wire corrosion-resistant drawing fluid according to claim 1, wherein: The lubricant is one or both of ester compounds and polyether compounds.

5. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 4, characterized in that: The HLB value of the polyether compound is less than 9.

6. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 4, characterized in that: The ester compound is triethanolamine oleate, and the polyether compound is trans-block polyether.

7. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 1, characterized in that: The low carbonic acid is one or more of neodecanoic acid, isononanoic acid and isodecanoic acid.

8. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 1, characterized in that: The corrosion inhibitor is one or more of benzotriazole, methylbenzotriazole, 1-hydroxymethylbenzotriazole, 1-benzotriazole-methyl methacrylate, poly(1-benzotriazole-methyl methacrylate-methyl acrylate) and poly(1-benzotriazole-methyl methacrylate-acrylic acid).

9. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 8, characterized in that: The corrosion inhibitor is benzotriazole.

10. The method for improving the lubrication and cleaning properties of copper wire corrosion-resistant drawing fluid according to claim 1, characterized in that: The wetting agent is an acetylene alcohol surfactant.

Citation Information

Cited By

  • Low-carbon total-synthesis roller grinding fluid

    CN119899725A