A high-strength new energy motor copper wire and preparation method thereof

Through the combination of Fe-Co-Al medium entropy alloy and Ni3Al alloy, the alloy grains are refined, and the metallographic structure of copper-aluminum alloy is improved, the contradiction between mechanical strength and conductive properties of copper wire is solved, and high strength and high conductivity are achieved. The preparation of copper wire for new energy motors reduces costs.

CN118595447BActive Publication Date: 2024-11-19GUANGDONG HUACHUANGYING HARDWARE TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410863188.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-29
Publication Date
2024-11-19
Estimated Expiration
2044-06-29

AI Technical Summary

Technical Problem

While improving the mechanical strength of copper wires, the conductivity performance decreases, making it difficult to maintain high conductivity under the premise of cost control.

Method used

Using Fe-Co-Al medium entropy alloy and Ni3Al alloy as reinforced phase and bonded phase, high-strength new energy motor copper wire is prepared through high-energy ball milling, vacuum arc smelting and hybrid smelting, and the alloy grains are refined to improve copper and aluminum. Alloy metallographic structure improves mechanical strength and electrical conductivity.

Benefits of technology

The mechanical strength and conductivity of copper wires are significantly improved, and the cost is reduced. At the same time, the addition of Ni3Al alloys suppresses the deterioration of conductivity caused by entropy alloys in Fe-Co-Al, which enhances the density degree of alloy and the crystal structure arrangement of the alloys. Tightness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004919511740000041
    Figure BDA0004919511740000041
Patent Text Reader

Abstract

The present invention belongs to the technical field of conductive materials and alloys, and discloses a high-strength copper wire for new energy motors and a preparation method thereof. The preparation method comprises the following steps: (1) mixing Fe, Co, and Al single substance powders in a molar ratio of 0.95-1.05:0.95-1.05:0.95-1.05 and then subjecting the mixture to high-energy ball milling to obtain Fe‑Co‑Al medium entropy alloy powder; (2) subjecting the obtained Fe‑Co‑Al medium entropy alloy powder to vacuum arc melting or discharge plasma sintering to obtain Fe‑Co‑Al medium entropy alloy; (3) subjecting the Fe‑Co‑Al medium entropy alloy to mixed melting, stretching, and annealing with Ni3Al alloy, copper ingot, and aluminum ingot to obtain high-strength copper wire for new energy motors. The present invention uses aluminum alloy to strengthen the copper wire, which can significantly improve the strength and conductivity of the copper-aluminum alloy, can be applied to high-power new energy motors, and has the advantages of high strength and high stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of conductive materials and alloys, and in particular relates to a high-strength new energy motor copper wire and a preparation method thereof. Background Art

[0002] New energy vehicles have become an important direction for the development of future vehicles, and motors are their core power. Copper wire is an important part of the motor, mainly used for the conduction of the motor. Copper wire has excellent properties such as good conductivity and ductility, and is a necessary part for transmitting electrical energy inside the motor. In modern motors, as the power of the motor gradually increases, the proportion of copper wire also gradually increases. For high-power motors, the proportion of copper wire can often reach more than 20%.

[0003] However, the mechanical strength of pure copper wire is not high, and the cost of pure copper wire is relatively high, so the development of copper wire for new energy motors with higher mechanical strength and lower cost has broad market prospects. In the prior art, aluminum-copper alloy is used to replace pure copper. This aluminum-copper alloy wire has high strength, but its conductivity and stability performance when used in high-power new energy motors are seriously reduced.

[0004] WO 2017 / 080068 A1 discloses a copper-aluminum alloy for cable materials, and the addition of each element is calculated by weight, and its composition is: Cu: 40-60 parts, Zn: 6-12 parts, Ni: 6-18 parts, Si: 2-8 parts, Fe: 2-4 parts, and the rest is AI and impurities that cannot be removed. The obtained cable material has low resistance, strong conductivity, and also enhances the tensile strength of the material. At the same time, the Ni in the composition effectively enhances the corrosion resistance of the material, and has excellent bending processing performance and stress relaxation characteristics. CN109360679A discloses an aluminum-copper alloy wire, which is made of an alloy material with a mass percentage of copper 10-20%, silver 1-2%, magnesium 0.2-0.5%, silicon 0.2-0.5%, cobalt 0.05-0.2%, and the remainder is aluminum. CN 105261406 A discloses a high-strength copper wire, which comprises Cu, Sn, Si, Zn and Al, wherein the proportion of Cu accounts for 70-80% of the total mass, the proportion of Sn accounts for 0.5-0.8% of the total mass, the proportion of Si accounts for 0.1-0.5% of the total mass, the proportion of Zn accounts for 10-15% of the total mass, and the balance is Al.

[0005] It can be seen from the above prior art that the main method to improve the mechanical strength and reduce the cost of copper wire is to add aluminum alloy. However, due to the differences in crystal structure, atomic radius and electronegativity between copper and aluminum, the enhancement effect on mechanical strength is relatively limited. At the same time, the addition of aluminum alloy has a significant adverse effect on the conductivity of copper wire. Therefore, how to improve the mechanical properties of copper alloy while maintaining its high conductivity is a technical problem that technicians in this field need to solve. Summary of the invention

[0006] In view of the shortcomings and deficiencies of the above prior art, the primary purpose of the present invention is to provide a method for preparing high-strength new energy motor copper wire.

[0007] Another object of the present invention is to provide a high-strength new energy motor copper wire prepared by the above method.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A method for preparing a high-strength new energy motor copper wire comprises the following preparation steps:

[0010] (1) mixing Fe, Co, and Al powders in a molar ratio of 0.95-1.05:0.95-1.05:0.95-1.05 and then high-energy ball milling to obtain Fe-Co-Al medium entropy alloy powder;

[0011] (2) subjecting the obtained Fe-Co-Al medium entropy alloy powder to vacuum arc melting or spark plasma sintering to obtain a Fe-Co-Al medium entropy alloy;

[0012] (3) The Fe-Co-Al medium entropy alloy is mixed with Ni3Al alloy, copper ingots and aluminum ingots through mixed smelting, stretching and annealing to obtain high-strength new energy motor copper wire.

[0013] Preferably, the average particle size of the Fe, Co and Al single substance powders in step (1) is ≤50 μm, and the purity is >99.9%.

[0014] Preferably, the high-energy ball milling in step (1) refers to ball milling for 4 to 12 hours at a ball-to-material ratio of 8 to 15:1 and a rotation speed of 300 to 500 r / min.

[0015] Preferably, the temperature of the vacuum arc melting or spark plasma sintering in step (2) is 1100-1400°C.

[0016] Preferably, the mass percentages of the mixed smelting of the Fe-Co-Al medium entropy alloy, Ni3Al alloy, copper ingot and aluminum ingot in step (3) are: 3% to 8% of the Fe-Co-Al medium entropy alloy, 1% to 5% of the Ni3Al alloy, 47% to 70% of the copper ingot and 26% to 40% of the aluminum ingot.

[0017] Further preferably, the mass ratio of the Ni3Al alloy to the Fe-Co-Al medium entropy alloy is 1 to 2:3.

[0018] Preferably, the temperature of the mixed smelting in step (3) is 1350-1550°C, and the temperature of the annealing is 550-650°C.

[0019] A high-strength new energy motor copper wire is prepared by the above method.

[0020] The principle of the present invention is: by adding aluminum to reduce the cost of copper wire, Fe-Co-Al medium entropy alloy and Ni3Al alloy are used as reinforcement phase and bonding phase to improve the metallographic structure of copper-aluminum alloy, refine the alloy grains, and improve the strength and conductivity of copper-aluminum alloy. However, the single Fe-Co-Al medium entropy alloy will lead to the deterioration of conductivity due to its lattice distortion effect. By using Ni3Al alloy as the bonding phase, on the one hand, nickel is dissolved in the copper matrix, dislocation and lattice distortion are reduced, and the defect of poor conductivity caused by Fe-Co-Al medium entropy alloy is reduced; on the other hand, it has good chemical compatibility with aluminum, can wet the grain boundary interface of copper-aluminum alloy, improve the relative densification degree of the alloy and the compactness of crystal structure arrangement, thereby improving the mechanical properties such as strength and conductivity of alloy copper wire.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention uses aluminum alloy to reinforce the copper wire, which can reduce the cost of the copper wire on the one hand and improve the mechanical strength of the copper wire on the other hand.

[0023] (2) The present invention uses Fe-Co-Al medium entropy alloy and Ni3Al alloy as reinforcement phase and bonding phase to improve the metallographic structure of copper-aluminum alloy, refine alloy grains, and improve the strength and conductivity of copper-aluminum alloy.

[0024] (3) The present invention uses Ni3Al alloy as a bonding phase, which, on the one hand, reduces the defect of poor conductivity caused by the lattice distortion effect of the Fe-Co-Al alloy crystal; on the other hand, it can wet the copper-aluminum alloy grain boundary interface, improve the relative densification degree of the alloy and the compactness of the crystal structure arrangement, thereby improving the mechanical properties and conductivity of the alloy copper wire such as strength. DETAILED DESCRIPTION

[0025] The present invention is further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto.

[0026] Example 1

[0027] A method for preparing a high-strength new energy motor copper wire comprises the following preparation steps:

[0028] (1) Fe, Co, and Al single-element powders with an average particle size of ≤50 μm and a purity of >99.9% were mixed in a molar ratio of 1:1:1 and added to a high-energy ball mill. The mixture was ball-milled for 8 h at a ball-to-material ratio of 10:1 and a rotation speed of 400 r / min to obtain Fe-Co-Al medium-entropy alloy powder.

[0029] (2) adding the Fe-Co-Al medium entropy alloy powder obtained in step (1) into a vacuum arc furnace for smelting at a smelting temperature of 1250-1300° C. for 90 min, and cooling the powder with the furnace after smelting to obtain a Fe-Co-Al medium entropy alloy.

[0030] (3) According to the mass percentage, 6% Fe-Co-Al medium entropy alloy and 3% Ni3Al alloy, 56% copper ingots and 35% aluminum ingots are added into a horizontal furnace for smelting at a smelting temperature of 1400-1500°C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 550-600°C. After cooling, it is wound by a rewinding machine to obtain high-strength new energy motor copper wire.

[0031] The copper wire obtained in this embodiment has a tensile strength of 252 MPa and an elongation of 18.1% according to a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 80.5% IACS.

[0032] The content of Ni3Al alloy in this embodiment is adjusted to 0%, 1%, 2%, 4%, 5% and 6% respectively. The test results of the copper wire performance obtained under different ratios of Fe-Co-Al medium entropy alloy and Ni3Al alloy are shown in Table 1 below. The control group is a copper-aluminum alloy without adding Fe-Co-Al medium entropy alloy and Ni3Al alloy reinforcement.

[0033] Table 1

[0034]

[0035] It can be seen from the results in Table 1 that the present invention can significantly improve the mechanical strength by strengthening the copper-aluminum alloy through the Fe-Co-Al medium entropy alloy, but the single Fe-Co-Al medium entropy alloy will significantly reduce the conductivity, which is due to the deterioration of conductivity caused by the lattice distortion effect of the Fe-Co-Al medium entropy alloy. By gradually increasing the content of Ni3Al alloy, the conductivity of the alloy is significantly improved, indicating that the addition of Ni3Al alloy has the effect of inhibiting the lattice distortion effect. The single Ni3Al alloy can improve the mechanical strength and conductivity to a certain extent, because it can wet the grain boundary interface of the copper-aluminum alloy as a bonding phase, improve the relative densification degree of the alloy and the compactness of the crystal structure arrangement, thereby improving the mechanical properties and conductivity. Under the same addition amount, the enhancement effect of the single Ni3Al alloy on the mechanical strength is significantly lower than that of the single Fe-Co-Al medium entropy alloy. Under the condition that the mass ratio of Ni3Al alloy to Fe-Co-Al medium entropy alloy is 1 to 2:3, good mechanical strength and conductivity can be achieved at the same time.

[0036] Example 2

[0037] A method for preparing a high-strength new energy motor copper wire comprises the following preparation steps:

[0038] (1) Fe, Co, and Al single-element powders with an average particle size of ≤50 μm and a purity of >99.9% were mixed in a molar ratio of 1:1:0.95 and added to a high-energy ball mill. The mixture was ball-milled for 4 h at a ball-to-material ratio of 8:1 and a rotation speed of 500 r / min to obtain Fe-Co-Al medium-entropy alloy powder.

[0039] (2) adding the Fe-Co-Al medium entropy alloy powder obtained in step (1) into a vacuum arc furnace for smelting at a smelting temperature of 1350-1400° C. for 120 min, and cooling the powder with the furnace after smelting to obtain a Fe-Co-Al medium entropy alloy.

[0040] (3) According to the mass percentage, 5% Fe-Co-Al medium entropy alloy and 2% Ni3Al alloy, 67% copper ingots and 26% aluminum ingots are added into a horizontal furnace for smelting at a smelting temperature of 1450-1550°C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 600-650°C. After cooling, it is wound by a rewinding machine to obtain high-strength new energy motor copper wire.

[0041] The copper wire obtained in this embodiment has a tensile strength of 220 MPa and an elongation of 19.6% according to a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 83.4% IACS.

[0042] Example 3

[0043] A method for preparing a high-strength new energy motor copper wire comprises the following preparation steps:

[0044] (1) Fe, Co, and Al single-element powders with an average particle size of ≤50 μm and a purity of >99.9% were mixed in a molar ratio of 1:1:1.05 and added to a high-energy ball mill. The mixture was ball-milled for 12 h at a ball-to-material ratio of 12:1 and a rotation speed of 300 r / min to obtain Fe-Co-Al medium-entropy alloy powder.

[0045] (2) adding the Fe-Co-Al medium entropy alloy powder obtained in step (1) into the heating chamber of the spark plasma sintering system, evacuating the chamber and performing spark plasma one-step liquid phase sintering at a sintering temperature of 1150-1200° C. for 8 min. cooling the chamber with the furnace after sintering to obtain the Fe-Co-Al medium entropy alloy.

[0046] (3) Calculated by mass percentage, 3% Fe-Co-Al medium entropy alloy and 1% Ni3Al alloy, 70% copper ingots and 26% aluminum ingots are added into a horizontal furnace for smelting at a smelting temperature of 1450-1550°C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 600-650°C. After cooling, it is wound by a rewinding machine to obtain high-strength new energy motor copper wire.

[0047] The copper wire obtained in this embodiment has a tensile strength of 206 MPa and an elongation of 20.5% according to a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 85.2% IACS.

[0048] Example 4

[0049] A method for preparing a high-strength new energy motor copper wire comprises the following preparation steps:

[0050] (1) Fe, Co, and Al single-element powders with an average particle size of ≤50 μm and a purity of >99.9% were mixed in a molar ratio of 0.95:1:1.05 and added to a high-energy ball mill. The mixture was ball-milled for 8 h at a ball-to-material ratio of 10:1 and a rotation speed of 400 r / min to obtain Fe-Co-Al medium-entropy alloy powder.

[0051] (2) adding the Fe-Co-Al medium entropy alloy powder obtained in step (1) into the heating chamber of the spark plasma sintering system, evacuating the chamber and performing spark plasma one-step liquid phase sintering at a sintering temperature of 1150-1200° C. for 5 min. cooling the chamber with the furnace after sintering to obtain the Fe-Co-Al medium entropy alloy.

[0052] (3) According to the mass percentage, 8% Fe-Co-Al medium entropy alloy and 5% Ni3Al alloy, 47% copper ingots and 40% aluminum ingots are added into a horizontal furnace for smelting at a smelting temperature of 1350-1400°C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 550-600°C. After cooling, it is wound by a rewinding machine to obtain high-strength new energy motor copper wire.

[0053] The copper wire obtained in this embodiment has a tensile strength of 289 MPa and an elongation of 15.1% according to a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 75.3% IACS.

[0054] Comparative Example 1

[0055] The preparation method of a high-strength new energy motor copper wire in this comparative example, compared with Example 2, does not pre-prepare Fe-Co-Al medium entropy alloy powder, and directly adopts single substance powder mixed smelting, and the specific preparation steps are as follows:

[0056] (1) Fe, Co, and Al single-substance powders with an average particle size of ≤50 μm and a purity of >99.9% are mixed in a molar ratio of 1:1:0.95 to obtain a mixed powder.

[0057] (2) Calculated by mass percentage, 5% of the mixed powder, 2% of the Ni3Al alloy, 67% of the copper ingot and 26% of the aluminum ingot are added into a horizontal furnace for smelting at a smelting temperature of 1450-1550° C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 600-650° C. After cooling, it is wound by a rewinding machine to obtain a copper wire.

[0058] The copper wire obtained in this comparative example has a tensile strength of 188 MPa and an elongation of 14.1% after a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 78.3% IACS.

[0059] By comparing the results of this comparative example with Example 2, it can be seen that if the Fe-Co-Al medium entropy alloy is not prepared by high-energy ball milling followed by smelting in advance, its strengthening effect on the copper-aluminum alloy is significantly reduced.

[0060] Comparative Example 2

[0061] In this comparative example, a method for preparing a high-strength new energy motor copper wire is disclosed. Compared with Example 2, Co is not added in the preparation process of the Fe-Co-Al medium entropy alloy. The specific preparation steps are as follows:

[0062] (1) Fe and Al single-substance powders with an average particle size of ≤50 μm and a purity of >99.9% were mixed in a molar ratio of 1:0.95 and added to a high-energy ball mill. The mixture was ball-milled for 4 h at a ball-to-material ratio of 8:1 and a rotation speed of 500 r / min to obtain Fe-Al alloy powder.

[0063] (2) adding the Fe-Al medium entropy alloy powder obtained in step (1) into a vacuum arc furnace for smelting at a smelting temperature of 1350-1400° C. for 120 min, and cooling with the furnace after smelting to obtain a Fe-Al alloy.

[0064] (3) Calculated by mass percentage, 5% Fe-Al alloy and 2% Ni3Al alloy, 67% copper ingot and 26% aluminum ingot are added into a horizontal furnace for smelting at a smelting temperature of 1450-1550° C. The smelted copper liquid is cooled by a condensing device, then pulled out by a traction mechanism, and then annealed at 600-650° C. After cooling, it is wound by a rewinding machine to obtain a copper wire.

[0065] The copper wire obtained in this comparative example has a tensile strength of 175 MPa and an elongation of 12.8% after a tensile test (GB / T 228-2010), and a conductivity test (International Conductive Copper Standard) of 74.6% IACS.

[0066] By comparing the results of this comparative example with those of Example 2, it can be seen that the use of Fe-Co-Al medium entropy alloy in combination with Ni3Al alloy significantly improves the reinforcement effect on copper-aluminum alloy.

[0067] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing high-strength new energy motor copper wire, characterized in that: The method comprises the following preparation steps: (1) Fe, Co, and Al single substance powders are mixed at a molar ratio of 0.95-1.05:0.95-1.05:0.95-1.05 and then subjected to high-energy ball milling to obtain Fe-Co-Al medium entropy alloy powder; (2) subjecting the obtained Fe-Co-Al medium entropy alloy powder to vacuum arc melting or spark plasma sintering to obtain a Fe-Co-Al medium entropy alloy; (3) The Fe-Co-Al medium entropy alloy is mixed with Ni3Al alloy, copper ingot and aluminum ingot for smelting, stretching and annealing to obtain high-strength copper wire for new energy motors; The mass percentages of the Fe-Co-Al medium entropy alloy, Ni3Al alloy, copper ingot and aluminum ingot mixed and smelted in step (3) are: 3% to 8% of the Fe-Co-Al medium entropy alloy, 1% to 5% of the Ni3Al alloy, 47% to 70% of the copper ingot and 26% to 40% of the aluminum ingot.

2. The method for preparing a high-strength new energy motor copper wire according to claim 1, characterized in that: The average particle size of the Fe, Co and Al single substance powders in step (1) is ≤50 μm, and the purity is >99.9%.

3. The method for preparing a high-strength new energy motor copper wire according to claim 1, characterized in that: The high-energy ball milling in step (1) refers to ball milling for 4 to 12 hours at a ball-to-material ratio of 8 to 15:1 and a rotation speed of 300 to 500 r / min.

4. The method for preparing a high-strength new energy motor copper wire according to claim 1, characterized in that: The temperature of the vacuum arc melting in step (2) is 1250-1400°C, and the temperature of the spark plasma sintering is 1150-1200°C.

5. The method for preparing a high-strength new energy motor copper wire according to claim 1, characterized in that: The mass ratio of the Ni3Al alloy to the Fe-Co-Al medium entropy alloy is 1-2:

3.

6. The method for preparing a high-strength new energy motor copper wire according to claim 1, characterized in that: The temperature of the mixed smelting in step (3) is 1350-1550°C, and the temperature of the annealing is 550-650°C.

7. A high-strength new energy motor copper wire, characterized in that: It is prepared by the method according to any one of claims 1 to 6.

Citation Information

Cited By

  • Copper alloy material, preparation method thereof and copper wire prepared from copper alloy material

    CN120843872A

  • Preparation process of high-strength and high-toughness copper wire

    CN121331560A

  • Preparation process of high-strength and high-toughness copper wire