Alloy steel for welding and smelting method thereof

By controlling the oxygen, manganese, sulfur and aluminum content in the molten steel and the addition time of alloying elements, semi-wrapped core-shell inclusions are formed, which solves the problem of insufficient low-temperature impact toughness of alloy steel for welding and achieves a significant improvement in welding performance. .

CN118755907APending Publication Date: 2024-10-11WUHAN UNIV OF SCI & TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410907691.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The low-temperature impact toughness of alloy steel for welding is low, and it is difficult to effectively improve it with existing technology.

Method used

By controlling the contents of oxygen, manganese, sulfur and aluminum in the molten steel, and controlling the addition time of calcium and other alloying elements during the alloying process, a semi-structured shell of TiN and MnS and a core of titanium-lanthanum-magnesium composite oxide is formed. Wrapped core-shell inclusions induce intragranular acicular ferrite nucleation, divide the grains and refine the weld structure, and improve the low-temperature impact toughness of welding.

Benefits of technology

The low-temperature impact toughness of alloy steel for welding is significantly improved, the impact energy reaches 63.7J~76.1J, and the welding performance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118755907A_ABST
    Figure CN118755907A_ABST
Patent Text Reader

Abstract

The invention discloses alloy steel for welding and a smelting method thereof. The technical problem that in the prior art, welding low-temperature impact toughness is low is solved. Comprising the following steps that molten steel with the mass fraction of oxygen ranging from 0.002% to 0.005%, the mass fraction of aluminum smaller than or equal to 0.003%, the mass fraction of sulfur ranging from 0.008% to 0.015% and the mass fraction of manganese ranging from 1.2% to 1.8% is obtained; and calcium alloy is added into the molten steel firstly, then titanium alloy, lanthanum alloy and magnesium alloy are added, alloying is achieved, and smelting is completed. The welding impact toughness of the alloy steel smelted by the smelting method provided by the invention is 63.7-76.1 J, and the welding impact toughness is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of alloy steel smelting, and specifically relates to an alloy steel for welding and a smelting method thereof. Background Art

[0002] Alloy steel for welding can be used in large structural parts in the fields of construction, marine engineering, energy storage, etc. after being welded using high-energy-input welding technology. However, the welding heat input is large, the peak temperature is high, and the peak temperature residence time is long during the high-energy-input welding process, and the mechanical properties of the welding heat-affected zone, especially the impact toughness, are significantly reduced.

[0003] In the related art, patent application CN103695777A discloses a thick steel plate with excellent toughness in the heat affected zone of welding and a manufacturing method thereof, which is characterized in that the number density of micron inclusions with a size of ≥1μm in the steel is controlled to be ≥60 / mm by designing the composition content of deoxidizing elements such as Ti, Al, Ca, REM, and Zr. 2 , and the Ca / Al ratio of inclusions is ≥0.10, the aspect ratio is ≤2.0; the number density of submicron inclusions with a size of <1μm is ≥300 / mm 2 Patent application CN105256095A discloses a method for smelting a steel plate with excellent performance in the heat-affected zone of high heat input welding, characterized in that 5<Ti / O<12 and (Mg+Zr) / (Ti+Al)>0.02 in the steel are controlled to form Mg-Ti, Zr-Ti, Mg-Zr-Ti composite inclusions with a size of less than 1μm in the steel, thereby improving the high heat input welding performance.

[0004] Although relevant technologies have provided technologies for improving the welding performance of high-wire energy welding of alloy steels, there is still room for improvement in the low-temperature impact toughness of welding. Summary of the invention

[0005] In order to solve the technical problem of low low-temperature impact toughness of alloy steel for welding, the present application provides an alloy steel for welding and a smelting method thereof.

[0006] In a first aspect of the present application, a method for smelting alloy steel for welding is provided, comprising the following steps:

[0007] Obtaining molten steel having an oxygen mass fraction of 0.002% to 0.005%, an aluminum mass fraction of less than or equal to 0.003%, a sulfur mass fraction of 0.008% to 0.015%, and a manganese mass fraction of 1.2% to 1.8%;

[0008] Calcium alloy is first added to the molten steel, and then titanium alloy, lanthanum alloy and magnesium alloy are added to achieve alloying and complete smelting.

[0009] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fraction ratio of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel is 0.8-1.2:15-25:12-18:1-5.

[0010] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fraction ratio of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel is 1:20:15:4.

[0011] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fractions of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel are 0.0010% to 0.0020%, 0.015% to 0.035%, 0.010% to 0.020% and 0.0010% to 0.0050%, respectively.

[0012] In some embodiments, after the calcium alloy is added to the molten steel, the titanium alloy, the lanthanum alloy and the magnesium alloy are added in sequence.

[0013] In some embodiments, there is a time interval of 5 min to 10 min between two adjacent alloys added to the calcium alloy, the titanium alloy, the lanthanum alloy and the magnesium alloy.

[0014] In some embodiments, the temperature is kept for 4 to 6 minutes after the magnesium alloy is added.

[0015] In some embodiments, the temperature of the molten steel is 1600°C to 1630°C.

[0016] In a second aspect of the present application, an alloy steel is provided, which is obtained by the smelting method of the welding alloy steel of the first aspect, and the alloy steel includes the following elements in mass fractions: calcium: 0.0010%~0.0020%, titanium: 0.015%~0.035%, lanthanum: 0.010%~0.020%, magnesium: 0.0010%~0.0050%, aluminum: ≤0.003%.

[0017] In some embodiments, in the alloy steel, the total mass fraction of calcium, titanium, lanthanum and magnesium is 0.045% to 0.125%.

[0018] According to the smelting method of the alloy steel for welding provided in the embodiment of the present application, the following steps are included: obtaining a steel liquid with a mass fraction of oxygen of 0.002% to 0.005%, a mass fraction of aluminum less than or equal to 0.003%, a mass fraction of sulfur of 0.008% to 0.015%, and a mass fraction of manganese of 1.2% to 1.8%; first adding a calcium alloy to the steel liquid, and then adding a titanium alloy, a lanthanum alloy and a magnesium alloy to achieve alloying and complete smelting. The present application forms a semi-encapsulated core-shell inclusion with an outer shell of TiN and MnS and an inner core of titanium lanthanum magnesium composite oxide inclusions by limiting the content of oxygen, manganese, sulfur and aluminum in the steel liquid and controlling the addition time of calcium elements and other alloying elements. The oxide inclusions in the semi-encapsulated core-shell inclusions can induce intracrystalline needle-shaped ferrite nucleation during the alloy steel welding process, which can effectively divide the grains, refine the organization of the weld and the heat-affected zone, and improve the welding low-temperature impact toughness of the weld and the heat-affected zone. In addition, a manganese-poor zone will be formed in the steel matrix near MnS during the solidification process, which enhances the ability of oxide inclusions in the semi-encapsulated core-shell inclusions to induce the nucleation of intracrystalline acicular ferrite, further improving the welding low-temperature impact toughness of the weld and the heat-affected zone. The welding impact toughness of the alloy steel smelted by the smelting method provided in this application is 63.7J~76.1J, and the welding impact toughness is good. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 A scanning electron microscope (SEM) image of the alloy steel of Example 1 of the present application is shown.

[0020] Figure 2 A scanning electron microscope (SEM) image of the alloy steel welding area of ​​Example 1 of the present application is shown.

[0021] Figure 3 An optical microscope (OM) image of the microstructure of the heat-affected zone of the alloy steel welding in Example 1 of the present application is shown.

[0022] Figure 4 A transmission electron microscope (TEM) image of the precipitation phase of the alloy steel in Example 1 of the present application is shown.

[0023] Figure 5 The SEM image of the alloy steel precipitation phase pinning the grain boundary in Example 1 of the present application is shown.

[0024] Figure 6 The optical microscope (OM) image of the microstructure of the heat affected zone of the alloy steel welding in Comparative Example 1 is shown. DETAILED DESCRIPTION

[0025] In order to make the technical personnel in the technical field to which the present application belongs to understand the present application more clearly, the technical scheme in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0026] The first aspect of the present application provides a method for smelting alloy steel for welding, which can improve the low-temperature impact toughness of the alloy steel for welding.

[0027] The smelting method of the alloy steel for welding provided in the embodiment of the present application comprises the following steps:

[0028] S1. Obtaining molten steel having an oxygen mass fraction of 0.002% to 0.005%, an aluminum mass fraction of less than or equal to 0.003%, a sulfur mass fraction of 0.008% to 0.015%, and a manganese mass fraction of 1.2% to 1.8%;

[0029] S2. Firstly, a calcium alloy is added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added to achieve alloying and complete smelting.

[0030] Oxygen is an element that forms oxide inclusions. Therefore, controlling the mass fraction of oxygen in the molten steel to 0.002% to 0.005% is conducive to the formation of composite oxide inclusions with the later added titanium, lanthanum and magnesium elements. This composite oxide inclusion can serve as the core for the precipitation of TiN and MnS during the solidification process, thereby forming semi-enclosed core-shell inclusions to improve the low-temperature impact toughness of the weld and the heat-affected zone. If the mass fraction of oxygen is lower than 0.002%, the number of semi-enclosed core-shell inclusions will be reduced to a certain extent, which is not conducive to the induction of intracrystalline needle-shaped ferrite nucleation during the welding process, thereby affecting the low-temperature impact toughness of the weld and the heat-affected zone. If the mass fraction of oxygen is higher than 0.005%, the formed steel may have defects such as bubbles and looseness, and the strength, plasticity, hardness, impact toughness, etc. of the weld will be greatly reduced during welding.

[0031] Aluminum has a significant adverse effect on the formation of core-shell inclusions. The aluminum content is controlled to be ≤0.003%. During alloying, it can form calcium-aluminum composite inclusions with the added calcium element, which promotes the removal of aluminum-containing inclusions. If the mass fraction of aluminum is too high, titanium, lanthanum and magnesium in the molten steel will combine with aluminum to form aluminate inclusions of titanium, lanthanum and magnesium, which will largely prevent the formation of titanium, lanthanum and magnesium oxide inclusions in the molten steel. Such aluminate inclusions are not conducive to inducing the nucleation of intracrystalline needle-shaped ferrite during welding, thereby affecting the low-temperature impact toughness of the weld and the heat-affected zone.

[0032] Manganese and sulfur are the forming elements of the shell MnS of the semi-enclosed core-shell inclusions, which are controlled to be 1.2%≤Mn≤1.8%, and the sulfur content is 0.008%-0.015%. During the solidification of the molten steel, manganese can be combined with sulfur, and the composite oxide inclusions of La, Ti and Mg formed in the molten steel in the alloying stage are attached and precipitated on the surface to form a MnS shell. Since there is a manganese-poor area in the steel matrix around the MnS shell formed during the solidification process, the manganese-poor area can enhance the ability of the composite oxide inclusions of La, Ti and Mg to induce the formation of acicular ferrite, which is beneficial to increase the content of acicular ferrite in the weld and heat-affected zone, and further improve the welding low-temperature impact toughness of the weld and heat-affected zone. If the manganese content is too low, it is difficult for the outer layer of the composite oxide inclusions of La, Ti and Mg to form a manganese sulfide shell, which will also reduce the area of ​​the manganese-poor area, affecting the ability of the composite oxide inclusions of La, Ti and Mg to induce the formation of acicular ferrite. If the manganese content is too high, the formed manganese sulfide shell is easy to completely wrap the composite oxide inclusions of La, Ti and Mg, affecting the ability of the composite oxide inclusions of La, Ti and Mg to induce the formation of acicular ferrite.

[0033] During the alloying stage, calcium is added first, which will form calcium-aluminum composite inclusions with the aluminum element in the molten steel, which can accelerate the removal of aluminum inclusions in the steel. The titanium alloy, lanthanum alloy and magnesium alloy added later, the titanium element and lanthanum element will react with the oxygen element in the molten steel to form La-Ti-O inclusions, the magnesium element will react with the oxygen in the steel to form MgO, the formed La-Ti-O inclusions and MgO inclusions will collide in the molten steel to form a composite inclusion with one area being La-Ti-O inclusions and the other area being MgO inclusions, this composite oxide inclusion of La, Ti and Mg can be used as the core, during the solidification process of the molten steel, TiN first solidifies and precipitates on the outside of the composite oxide inclusion, and MnS solidifies and precipitates on the outside of the composite oxide inclusion later, thereby forming a semi-enclosed core-shell inclusion, this semi-enclosed core-shell inclusion will induce the nucleation of intracrystalline acicular ferrite during welding, effectively divide the grains, refine the structure of the weld and the heat-affected zone, thereby improving the welding low-temperature impact toughness of the weld and the heat-affected zone. At the same time, during the solidification process, a manganese-poor area will be formed in the steel matrix around the MnS shell. The manganese-poor area can enhance the ability of the composite oxide inclusions in the core-shell inclusions as the core to induce the nucleation of intracrystalline acicular ferrite during welding, thereby improving the welding low-temperature impact toughness of the weld and the heat-affected zone. In addition, part of the Ti element can form discretely distributed TiN and Ti x O yNano-pinning phase. Lanthanum is a rare earth element, which can form a discretely distributed rare earth nano-pinning phase during solidification and cooling. Mg can form discretely distributed nano-pinning phases MgO and MgN with N and O elements in the molten steel. The TiN and TiN formed above x O y , rare earth nano-pinning phase, MgO and MgN nano-pinning phase can play a pinning role, preventing the grain growth of the weld and heat-affected zone during high-temperature welding, and further improving the welding low-temperature impact toughness of the weld and heat-affected zone. In addition, MgO and MgN nano-pinning phases can also improve the stability of TiN and TiO2 nano-pinning phases, ensuring that TiN and TiO2 nano-pinning phases fully play a pinning role, so as to further improve the welding low-temperature impact toughness of the weld and heat-affected zone.

[0034] It can be seen from the above content that the present application forms a semi-enclosed core-shell inclusion with an outer shell of TiN and MnS and an inner core of titanium lanthanum magnesium composite oxide inclusions by limiting the content of oxygen, manganese, sulfur and aluminum in the molten steel and controlling the addition time of calcium and other alloying elements. The oxide inclusions in the semi-enclosed core-shell inclusions can induce intracrystalline needle-shaped ferrite nucleation during the alloy steel welding process, effectively divide the grains, refine the organization of the weld and the heat-affected zone, and improve the welding low-temperature impact toughness of the weld and the heat-affected zone. In addition, a manganese-poor zone will be formed in the steel matrix near MnS during the solidification process, and the manganese-poor zone enhances the ability of the oxide inclusions in the semi-enclosed core-shell inclusions to induce intracrystalline needle-shaped ferrite nucleation, further improving the welding low-temperature impact toughness of the weld and the heat-affected zone.

[0035] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fraction ratio of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel is 0.8-1.2:15-25:12-18:1-5.

[0036] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fraction ratio of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel is 1:20:15:4.

[0037] In some embodiments, a calcium alloy is first added to the molten steel, and then a titanium alloy, a lanthanum alloy and a magnesium alloy are added, so that the mass fractions of the calcium element, the titanium element, the lanthanum element and the magnesium element in the molten steel are 0.0010% to 0.0020%, 0.015% to 0.035%, 0.010% to 0.020% and 0.0010% to 0.0050%, respectively.

[0038] The calcium content is controlled at 0.0010% to 0.0020% to purify the molten steel, promote the removal of alumina inclusions, and disperse and refine the inclusions. If too much calcium is added, CaS inclusions are easily formed in the steel. On the one hand, CaS is easy to aggregate into large-sized inclusions, affecting the performance of the parent material, and on the other hand, it will affect the formation of a semi-enclosed shell structure of MnS in the outer layer of the oxide; if too little calcium is added, it is difficult to remove alumina.

[0039] The mass fraction of titanium is 0.015% to 0.035%, the mass fraction of lanthanum is 0.010% to 0.020%, and the mass fraction of magnesium is 0.0010% to 0.0050%. Within the above range, titanium, lanthanum and magnesium will form dispersed fine oxide inclusions and precipitation phases in the molten steel. The oxide inclusions of titanium, lanthanum and magnesium form the core of the core-shell inclusions, and TiN forms the shell of the core-shell inclusions and half wraps the core. And within the above range, the precipitation phase size of titanium, lanthanum and magnesium is concentrated in 10 to 50nm, in a dispersed state, which plays a pinning role, prevents the grain growth of the weld and the heat-affected zone during high-temperature welding, and further improves the welding low-temperature impact toughness of the weld and the heat-affected zone.

[0040] If there is too much titanium, large-sized TiN inclusions are easily formed during the solidification process, which affects the low-temperature impact toughness of the welding; if there is too little titanium, it is difficult to form TiN precipitation phase, which affects the low-temperature impact toughness of the welding.

[0041] If there is too much lanthanum, the alloy yield of titanium and magnesium will be affected because lanthanum has the strongest deoxidation ability. When the lanthanum content is too high, lanthanum phosphide or oxyphosphide may be formed in the steel, which is not conducive to inducing the formation of acicular ferrite and affecting the low-temperature impact toughness of welding. If the lanthanum content is too little, the rare earth oxides formed in the steel are limited, and the acicular ferrite induced by rare earth inclusions will be reduced, affecting the low-temperature impact toughness of welding.

[0042] If the magnesium content is too high, the reaction during the smelting process will be very violent, the alloy will be severely burned, and the alloy yield will be reduced; if the magnesium content is too low, the large-sized inclusions that can be carried away by the magnesium vapor during the smelting process will be limited, and the size of the inclusions in the steel will be relatively large, affecting the low-temperature impact toughness of the welding.

[0043] In some embodiments, after adding calcium alloy to the molten steel, the titanium alloy, the lanthanum alloy and the magnesium alloy are added in sequence, that is, titanium is added first, then lanthanum, and finally magnesium. Since La has the strongest deoxidation ability and rare earth inclusions are very easy to aggregate, La will first react with O and S in the molten steel to form a large number of fine dispersed rare earth inclusions when entering the molten steel. During the heat preservation process, the rare earth inclusions are significantly aggregated, and the size of the inclusions increases, resulting in a decrease in the toughness of the parent material, weld and heat-affected zone. If La is added first, the rare earth inclusions will gather for a long time, and the size of the inclusions in the steel will increase significantly. Mg has a low melting point, so magnesium will vaporize quickly after entering the molten steel. The floating Mg vapor can take away large-sized inclusions in the molten steel, so that the average size of the inclusions is reduced, which plays a role in controlling the size of the inclusions and purifying the molten steel. Therefore, Mg should be added last. If Mg is added first, the effect of molten steel purification is significantly reduced, and the number of large-sized inclusions in the molten steel increases, resulting in a decrease in the toughness of the parent material, weld and heat-affected zone. Therefore, magnesium is added last. Therefore, the appropriate order of addition is Ti→La→Mg.

[0044] In some embodiments, the addition time interval between two adjacent alloys of the calcium alloy, the titanium alloy, the lanthanum alloy and the magnesium alloy is 5 to 10 minutes, and each element can fully react within the time interval to form a composite oxide inclusion. After the lanthanum element is added, it can fully form oxide inclusions with titanium. After the magnesium element is added, it can fully refine the inclusions in the dispersed steel, and at the same time, it can form a composite oxide inclusion of titanium, lanthanum and magnesium as a core structure with the lanthanum titanium oxide inclusion.

[0045] In some embodiments, the magnesium alloy is kept warm for 4 to 6 minutes after being added. The purpose of the heat preservation is to allow the alloy to react completely in the molten steel on the one hand, and to allow magnesium vapor to float up and take away large-sized inclusions on the other hand, thereby controlling the size of the inclusions. If the heat preservation time is too long, the alloy will be severely burned, reducing the alloy yield.

[0046] In some embodiments, the temperature of the molten steel is 1600° C. to 1630° C. If the temperature of the molten steel is higher than the upper temperature limit, it may cause greater burnout of titanium, magnesium and lanthanum elements to a certain extent, and reduce the yield; if the temperature of the molten steel is lower than the lower temperature limit, the calcium element may be difficult to completely melt, affecting the yield.

[0047] A second aspect of the present application provides an alloy steel obtained by using the smelting method of the alloy steel for welding according to any embodiment of the first aspect, and the alloy steel has good welding low-temperature impact toughness.

[0048] In some embodiments, the alloy steel includes the following elements in mass fractions: calcium: 0.0010% to 0.0020%, titanium: 0.015% to 0.035%, lanthanum: 0.010% to 0.020%, magnesium: 0.0010% to 0.0050%, and aluminum: ≤0.003%.

[0049] In some embodiments, in the alloy steel, the total mass fraction of calcium, titanium, lanthanum and magnesium is 0.045% to 0.125%, or 0.030% to 0.060%.

[0050] The smelting method of the alloy steel for welding provided in the present application is further described in detail below in conjunction with specific embodiments.

[0051] Example 1 to Example 4

[0052] Step 1: Heat and melt the raw material Q345B steel (the composition is shown in Table 1, and the rest is Fe and inevitable impurities) in an induction furnace to 1600°C to 1630°C.

[0053] Step 2: After the raw steel is melted for 10 minutes, the calcium wire is fed into the induction furnace. After 5 to 10 minutes, Ti alloy, rare earth La and Fe-Mg alloy are added in sequence. The time interval between alloy additions is 5 minutes. After all alloys are added, keep warm for 5 minutes. At this time, the composition of the molten steel is as shown in the table, and the rest is Fe and unavoidable impurities.

[0054] Step 3: Pour the molten steel obtained in step 3 into a steel ingot mold in a vacuum furnace and cool it to room temperature to obtain alloy steel.

[0055] Comparative Example 1

[0056] Q345B steel (with the same composition as in Example 1) was heated and melted in an induction furnace to 1600°C, and then introduced into an ingot mold in a vacuum furnace and air-cooled to room temperature to obtain alloy steel.

[0057] Comparative Example 2

[0058] Comparative Example 2 is based on Example 1. The difference between Comparative Example 2 and Example 1 is that in step 2, Fe-Mg alloy is added first, and then rare earth La, Ca wire and Ti alloy are added in sequence.

[0059] Table 1 Chemical composition of raw materials

[0060] Table 2 Chemical composition of alloy steel serial number Calcium Titanium Lanthanum Magnesium Example 1 0.0010% 0.025% 0.018% 0.0046% Example 2 0.0011% 0.015% 0.010% 0.0010% Example 3 0.0008% 0.020% 0.016% 0.0032% Example 4 0.0012% 0.022% 0.013% 0.0025% Comparative Example 1 0 0 0 0 Comparative Example 2 0.0012% 0.018% 0.020% 0.0035%

[0061] Table 3 Chemical composition of alloy steel (continued from Table 2) serial number C / % Si / % Mn / % S / % O / % <![CDATA[Al s / %]]> N / % Example 1 0.16 0.30 1.50 0.0095 0.0032 0.003 0.0046 Example 2 0.16 0.30 1.50 0.0095 0.0032 0.003 0.0052 Example 3 0.16 0.30 1.60 0.012 0.0036 0.0028 0.0064 Example 4 0.16 0.30 1.50 0.012 0.0045 0.0030 0.0064 Comparative Example 1 0.16 0.30 1.50 0.0095 0.0062 0.003 0.0046 Comparative Example 2 0.16 0.30 1.50 0.0102 0.0038 0.003 0.0048

[0062] After the riser of the alloy steel ingot was cut off, it was kept in a soaking furnace at 1200℃ for 3h for component annealing. Then the ingot was rolled into a plate with a thickness of 15mm using the TMCP process, with the start rolling at 1100℃ and the final rolling at 900℃. After rolling, the steel plate was cooled to room temperature at a cooling rate of 15℃ / min. Then the two alloy steel plates were butt welded, and a standard impact specimen was taken from the weld, with the "V"-shaped groove located on the weld point. After the temperature was controlled at -20℃ and kept for 30min, the Charpy impact test was carried out using a ZBC2452-3 pendulum impact tester. The results are shown in Table 3.

[0063] Table 4 Low temperature impact toughness serial number Impact toughness / J Example 1 76.1 Example 2 68.2 Example 3 66.9 Example 4 63.7 Comparative Example 1 2.7 Comparative Example 2 35.6

[0064] Figure 1 The scanning electron microscope (SEM) image of the alloy steel of Example 1 of the present application is shown, combined with Figure 1 It can be seen that a semi-enclosed core-shell inclusion is formed in the alloy steel, with the titanium-lanthanum-magnesium composite oxide inclusion as the center and MnS and TiN enclosed outside the center.

[0065] Figure 2 The SEM image of the alloy steel welding area of ​​Example 1 of the present application is shown. Figure 2 It can be seen that the acicular ferrite is induced to form during the welding process, which can improve the welding impact toughness of the alloy steel.

[0066] From the data in Table 4, it can be seen that the welding impact toughness of the alloy steel provided in Examples 1 to 4 of the present application is 63.7J to 76.1J, and the welding impact toughness is good. The welding impact toughness of the alloy steel provided in Comparative Example 1 of the present application is 2.7J, which is not as good as that of the present application. The welding impact toughness of the alloy steel provided in Comparative Example 2 of the present application is 35.6J, which is not as good as that of the present application.

[0067] In the present application, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0068] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise" and "counterclockwise" indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0069] In this application, unless otherwise clearly specified and limited, the terms "connection", "fixation", etc. should be understood in a broad sense. For example, "fixation" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0070] In addition, the descriptions of "first", "second", etc. in this application are only for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include one or more features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0071] Although the embodiments of the present application have been shown and described, those skilled in the art will appreciate that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the claims and their equivalents.

Claims

1. A method for smelting alloy steel for welding, characterized in that: The steps include: Obtaining molten steel having an oxygen mass fraction of 0.002% to 0.005%, an aluminum mass fraction of less than or equal to 0.003%, a sulfur mass fraction of 0.008% to 0.015%, and a manganese mass fraction of 1.2% to 1.8%; Calcium alloy is first added to the molten steel, and then titanium alloy, lanthanum alloy and magnesium alloy are added to achieve alloying and complete smelting.

2. The smelting method of alloy steel for welding according to claim 1, characterized in that: Calcium alloy is first added to the molten steel, and then titanium alloy, lanthanum alloy and magnesium alloy are added, so that the mass fraction ratio of calcium element, titanium element, lanthanum element and magnesium element in the molten steel is 0.8-1.2:15-25:12-18:1-5.

3. The smelting method of alloy steel for welding according to claim 2, characterized in that: Calcium alloy is first added to the molten steel, and then titanium alloy, lanthanum alloy and magnesium alloy are added, so that the mass fraction ratio of calcium element, titanium element, lanthanum element and magnesium element in the molten steel is 1:20:15:

4.

4. The smelting method of alloy steel for welding according to claim 2, characterized in that: Calcium alloy is first added to the molten steel, and then titanium alloy, lanthanum alloy and magnesium alloy are added, so that the mass fractions of calcium element, titanium element, lanthanum element and magnesium element in the molten steel are 0.0010% to 0.0020%, 0.015% to 0.035%, 0.010% to 0.020% and 0.0010% to 0.0050% respectively.

5. The method for smelting alloy steel for welding according to any one of claims 1 to 4, characterized in that: After adding the calcium alloy to the molten steel, the titanium alloy, the lanthanum alloy and the magnesium alloy are added in sequence.

6. The method for smelting alloy steel for welding according to claim 5, characterized in that: Among the calcium alloy, the titanium alloy, the lanthanum alloy and the magnesium alloy, there is a time interval of 5 minutes to 10 minutes between two adjacent alloys added.

7. The method for smelting alloy steel for welding according to claim 6, characterized in that: After adding the magnesium alloy, the temperature is kept at 4 to 6 minutes.

8. The method for smelting alloy steel for welding according to any one of claims 1 to 4, characterized in that: The temperature of the molten steel is 1600°C to 1630°C.

9. An alloy steel, characterized in that: The alloy steel is obtained by the smelting method of the welding alloy steel according to any one of claims 1 to 8, wherein the alloy steel comprises the following elements in mass fraction: calcium: 0.0010% to 0.0020%, titanium: 0.015% to 0.035%, lanthanum: 0.010% to 0.020%, magnesium: 0.0010% to 0.0050%, and aluminum ≤0.003%.

10. The alloy steel according to claim 9, characterized in that: In the alloy steel, the total mass fraction of calcium, titanium, lanthanum and magnesium is 0.045% to 0.125%.

Citation Information

Patent Citations

  • Thick steel plate with excellent tenacity for excellent-tenacity welding heat affected zone and manufacturing method thereof

    CN103695777A

  • Method for smelting steel plate with excellent performance in high-heat-input-welding heat affected zone

    CN105256095A