High-strength rare earth modified aluminum alloy material and preparation method thereof
By adding rare earth elements and Zr to aluminum alloys, nanoparticles with high stability are formed, and the process is optimized to solve the shortcomings in strength and hardenability of existing aluminum alloy materials and achieve high strength and fatigue resistance. Improvement to meet high-performance requirements in aviation, rail transit, automobiles and other fields.
Patent Information
- Application Number
- CN202410918463.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-11
AI Technical Summary
Existing aluminum alloy materials are insufficient in performance, especially in terms of strength and hardenability, and fail to meet the high requirements of aviation, rail transit, automobiles and other fields. In particular, research on super-strong aluminum alloys (800MPa strength level) is still being pursued. middle.
Using high-strength rare earth modified aluminum alloy materials, by adding rare earth elements, Zr, Ti and other elements, high-density and stable L12 structure Al3 (RE, Zr) nanoparticles are formed, and through a composite strengthening equal multi-level mechanism of action, it improves Mechanical properties and stress corrosion resistance of the alloy, while optimizing the chemical composition and process flow, including smelting, homogenization treatment, hot extrusion and aging treatment, and controlling the microstructure and component distribution of the alloy.
It significantly improves the tensile strength, yield strength and elongation after fracture of aluminum alloys, meets the demand for high-strength and lightweight materials, and improves the comprehensive properties of the material, including mechanical properties and fatigue resistance.
Smart Images

Figure CN118756017A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-strength rare earth modified aluminum alloy material and a preparation method thereof, belonging to the technical field of aluminum alloy material preparation. Background Art
[0002] High-strength and high-toughness aluminum alloy (Al-Zn-Mg-Cu system) has the characteristics of light weight, high strength, good toughness, etc., and has a very wide range of applications. It is achieved by adding an appropriate amount of other alloying elements to metal aluminum so that it has excellent comprehensive properties and can replace some heavy metal materials to achieve the purpose of lightweighting. As aircraft continue to develop along the trend of large-scale, the requirements for aluminum alloys are also constantly increasing. Not only do they need to have good strength and toughness, but they also need to have high hardenability. It also has good application prospects in high-strength structural parts such as the field of automotive safety protection (bumpers, anti-collision beams). Super-strong aluminum alloys, especially super-strong aluminum alloys with a strength level of 800MPa, have always been the goal pursued by researchers.
[0003] Therefore, it is very necessary to develop higher performance Al-Zn-Mg-Cu alloys for aviation materials, rail transit and automotive lightweight materials. Summary of the invention
[0004] In view of the shortcomings of existing aluminum alloy materials in performance, the first purpose of the present invention is to provide a high-strength rare earth modified aluminum alloy material. The high-strength rare earth modified aluminum alloy material provided by the present invention has higher strength and can be used as a lightweight material in aviation, rail transportation, and automobiles.
[0005] The second object of the present invention is to provide a method for preparing a high-strength rare earth modified aluminum alloy material.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The invention provides a high-strength rare earth modified aluminum alloy material, which has the following chemical components by mass percentage: Mn 0.2-1.0%, Cu 1.0-1.5%, Zn 9.5-10.5%, Mg 2.0-3.0%, Zr 0.05-0.3%, Ti 0-0.3%, RE 0.05-0.4%, and the balance is Al and inevitable impurities.
[0008] The aluminum alloy material provided by the present invention is added with rare earth elements, and the unique electronic structure characteristics of the rare earth elements are utilized to have the effects of purification, refinement, modification, microalloying, activation, etc. in the aluminum alloy. Due to the high activity, the rare earth elements are very easy to react with oxygen, hydrogen, sulfur, and nitrogen in the aluminum alloy to form corresponding stable compounds, which can purify the alloy. The solubility of the rare earth elements in the aluminum alloy is relatively low, and most of them are gathered in the liquid phase boundary layer at the front of the interface, which significantly increases the amount of the second phase, and the second phase is distributed at the grain boundary and between the α dendrites, playing a role in grain boundary strengthening. When RE and Zr are added in combination, Al3(RE, Zr) nanoparticles with L12 structure with high density and high temperature stability appear in the alloy. They are coherent or semi-coherent with the matrix, and have the characteristics of high melting point and good stability. In addition, a large number of fine, dispersed, petal-shaped secondary Al3(RE, Zr) particles are precipitated during the homogenization annealing process, which can pin dislocations and subgrain boundaries, effectively inhibit the migration of dislocations and promote the fixation of subgrain boundaries, hinder the migration of subgrain boundaries and the length of subgrains, and show better anti-recrystallization ability. By forming a multi-level action mechanism such as a composite strengthening phase, the mechanical properties and stress corrosion resistance of the alloy are effectively improved.
[0009] The high-strength rare earth modified aluminum alloy material of the present invention adopts a higher main element content, wherein the main elements include three elements of Zn, Mg, and Cu, which are also the main strengthening elements, and will form η phase, S phase and T phase in the alloy, which play a strengthening role on the strength of the alloy, wherein η phase (MgZn2) is the main strengthening phase, and generally speaking, increasing the mass percentage of Zn and Mg in the alloy can increase the number of η phases, thereby improving the strength of the alloy material. The strengthening effect of T phase (Al2Mg2Zn3) is slightly inferior, and when the Zn / Mg ratio is small, the main precipitation phase is T phase, and the main strengthening phase (η phase) is relatively small. The strengthening effect of S phase (Al2CuMg) is weaker, and has a supplementary strengthening effect on the alloy, mainly by refining the precipitation phase to make its distribution dispersed, thereby enhancing the aging strengthening effect of the alloy, and improving the fracture toughness and corrosion resistance of the alloy.
[0010] However, in the present invention, the amount of each component needs to be effectively controlled. If the Zn / Mg value of the alloy is increased, the alloy recrystallization and grain growth will be promoted. Properly increasing the Zn / Mg value in the alloy will play a strong hardening role, but when it exceeds a certain limit, the strength will decrease. With the increase of Cu / Mg, Cu will generate S phase with Mg and Zn, so that the amount of MgZn2 strengthening phase is reduced. In addition, the increase of Cu / Mg value will promote the recovery recrystallization of the alloy, and the grains will grow significantly, thereby reducing the strength, but improving the toughness of the alloy.
[0011] Furthermore, the high-strength rare earth modified aluminum alloy material has the following chemical composition, calculated by mass percentage: Mn 0.3-0.8%, Cu 1.0-1.5%, Zn 9.5-10.5%, Mg 2.0-3.0%, Zr 0.05-0.3%, Ti 0.02-0.1%, RE 0.05-0.4%, and the remainder is Al and unavoidable impurities.
[0012] Furthermore, the RE is selected from at least one of Sc, La, Ce, Y, Yb, and Er.
[0013] Furthermore, the high-strength rare earth modified aluminum alloy material, the aluminum alloy has a tensile strength Rm≥820MPa, a yield strength Rp0.2≥800Mpa, and an elongation after fracture A≥6% under T651 heat treatment.
[0014] In the present invention, among the inevitable impurities, the Si content in the aluminum alloy is less than 0.08%, the Fe content is less than 0.12%, the content of a single other element is less than 0.05%, and the combined content of other elements is less than 0.15%.
[0015] The present invention also provides a method for preparing a high-strength rare earth modified aluminum alloy material, comprising the steps of: smelting various metal raw materials according to a designed ratio to obtain a melt, casting the melt to obtain an ingot, homogenizing the ingot to obtain a homogenized billet, hot extruding the homogenized billet to obtain an extruded billet, and heat treating the extruded billet to obtain an aluminum alloy material.
[0016] In the present invention, alloy elements Mn, Cu, Zr and RE are added in the form of intermediate alloys Al-Mn, Al-Cu, Al-Zr and Al-RE respectively, Ti is added to the alloy in the form of Al-Ti-C, and Zn and Mg are pure zinc ingots and pure magnesium ingots to minimize the segregation of alloy elements in the ingot.
[0017] Furthermore, scrap aluminum, recycled materials, pure zinc, pure magnesium, pure zinc, Al-10Mn, Al-20Cu, Al-4Zr and Al-5RE are prepared according to the designed proportion.
[0018] In the present invention, Al-10Mn means that the molar fraction of Mn in Al-10Mn is 10%, Al-20Cu means that the molar fraction of Cu in Al-20Cu is 20%, Al-4Zr means that the molar fraction of Zr in Al-4Zr is 4%, and Al-5RE means that the molar fraction of RE in Al-5RE is 5%.
[0019] The inventors have found that the use of the above raw materials can significantly reduce the segregation of alloy elements in ingots.
[0020] Furthermore, the smelting process is to first throw the crushed aluminum and the recycled materials into the bottom of the furnace, put the aluminum ingots thereon, melt them to obtain aluminum liquid, and then uniformly add Al-20Cu, Al-4Zr, Al-10Mn, Al-10RE intermediate alloy, Zn ingot, and Mg ingot in sequence to obtain aluminum alloy liquid, stir, and when the temperature of the aluminum alloy liquid is 730-750°C, skim the slag, and after the composition is qualified, use argon gas for refining, the refining temperature is 730-740°C, and the refining time is 15-20min.
[0021] In the smelting process of the present invention, crushed aluminum and small recycled aluminum are first thrown into the furnace bottom when loading the furnace to protect the furnace bottom. After other materials are put in successively, they are strictly prohibited from being exposed to the liquid surface or close to the furnace bottom.
[0022] Furthermore, the casting is semi-continuous casting, the casting temperature is controlled at 690-710° C., Al-5Ti-0.2C wire is connected, double wire feeding is adopted, and the speed is 35-45 mm / min.
[0023] In actual operation, the filter plate adopts 30ppi+50ppi double-stage filtration during casting.
[0024] Furthermore, the homogenization process is to uniformly heat the ingot to 400-420°C within 1.5-2 hours, then keep the temperature for 5-8 hours, and then heat the ingot to 450-460°C again, and keep the temperature for 18-20 hours. The homogenization process can reduce the presence of compounds in the microstructure of the ingot after the ingot is heated.
[0025] The alloy of the present invention has a relatively high content of Zn, Cu and Mg elements, which will lead to the generation of a large number of dendrites in the alloy matrix and the occurrence of regional segregation. At this time, more intermetallic compounds and some non-equilibrium eutectic structures will appear. Moreover, during the crystallization process of the alloy, due to the changes in cooling intensity and temperature, internal stress and component segregation exist in the structure of the ingot after crystallization and cooling, and these defects will be inherited to the subsequent processing process, thereby affecting various properties of the alloy, especially the mechanical properties; therefore, the present invention adopts a two-stage homogenization treatment system, firstly raising the pretreatment temperature to 400-420°C, which not only plays a stress relief role, but also promotes the dispersion and precipitation of the LI2 type structure Al3 Zr phase, which can increase the recrystallization temperature of the alloy in the subsequent thermal deformation process, reduce the recrystallization ratio, and play a role in improving the performance of the alloy, and then using the secondary high temperature (450-460°C) for a long time to keep warm is mainly to eliminate component segregation, make the alloy elements evenly distributed, ensure that the low melting point second phase is dissolved into the matrix, and form a supersaturated solid solution, so as to provide sufficient solute atoms for subsequent aging treatment; furthermore, the gradual homogenization can well avoid the risk of overburning of the alloy due to temperature error.
[0026] Furthermore, the hot extrusion is forward hot extrusion. During the hot extrusion, the preheating temperature of the homogenized billet is 410-450°C, the preheating and holding time of the homogenized billet is 75-120 minutes, the preheating temperature of the mold is 420-460°C, the preheating and holding time of the mold is 120-240 minutes, and the extrusion rate is 0.5-4 mm / s.
[0027] In the present invention, by controlling the parameters of hot extrusion within the above range, the performance of the alloy material finally obtained is optimal. If the preheating temperature and time are too low, the deformation resistance during the extrusion process is large and the extrusion cannot be performed; if the preheating temperature and time are too high, the ingot will be overburned, the performance will be reduced, or cracks will appear. If the extrusion speed is too low, the production efficiency is low, the ingot cooling deformation resistance is large, and the extrusion cannot be performed; if the speed is too fast, cracks such as edge cracks will occur.
[0028] Furthermore, the heat treatment process is to first subject the extruded billet to a solution treatment, then to a stretching deformation treatment, and then to an aging treatment.
[0029] Furthermore, the process of the solution treatment is: firstly heating to 410-420°C at a rate of 50-100°C / h, keeping warm for 1-1.5h, heating to 465-472°C again, keeping warm for 1.5-2h, then taking out the extruded billet and transferring it to water, controlling the transfer time to be less than 10s.
[0030] In actual operation, the extruded billet is transferred to water at 20-35°C (normal temperature), and then the extruded billet is dried before being stretched and deformed.
[0031] Furthermore, the stretching deformation amount of the stretching deformation treatment is 1.5-3%.
[0032] Furthermore, the aging treatment temperature is 115-125° C., and the aging treatment time is 20-26 hours.
[0033] In the Al-Zn-Mg-Cu alloy provided in the present invention, due to the high content of alloying elements and non-equilibrium crystallization, there is inevitably an undissolved eutectic phase. Therefore, the present invention uses a two-stage solid solution treatment. First, a low-temperature solid solution process is performed to promote the diffusion of the non-equilibrium phase and allow the low-melting-point eutectic phase to dissolve in the matrix. Without overburning, the temperature is increased again and kept warm for a period of time to allow the high-melting-point crystalline phase to fully dissolve, and finally a solid solution with a higher supersaturation is obtained, thereby generating more precipitated phases through aging decomposition to hinder dislocation movement, strengthen the material, and obtain higher mechanical properties.
[0034] In addition, the present invention adds a stretching deformation treatment before the aging treatment. This is because a large amount of residual stress will be formed inside the material after the solution quenching treatment. The residual stress inside the alloy material is redistributed and tends to be uniform by applying 1.5% to 3% plastic deformation through a stretching machine. Moreover, after the stretching deformation before aging, a large number of dislocations introduced provide a large number of nucleation particles for subsequent aging precipitation, promote aging precipitation, and accelerate the aging response speed. At the same time, increasing the cold deformation amount after the solution quenching is conducive to shortening the time to reach the peak aging, improving the aging peak effect and saving industrial production costs. The pre-deformation can not only effectively reduce or eliminate the residual stress, but also the dislocations introduced by the pre-deformation also promote the increase of the aging precipitation phase, thereby affecting the fatigue performance and mechanical properties of the alloy.
[0035] The inventors found that if a single-stage solid solution is adopted, the solid solution temperature is too low and the residual crystalline phase cannot be fully dissolved in the matrix. If the temperature is too high, it will easily cause the alloy to be overburned. Under the condition of no overburning, a single temperature is used for solid solution treatment, and the transformation of the non-equilibrium multiphase structure into the solid solution structure is not complete, thereby affecting the mechanical properties and corrosion properties of the alloy.
[0036] In addition, during the solution quenching transfer process, the extruded billet needs to be quickly transferred to the water. If the speed is too slow, the material will come into contact with cold air during the transfer to the quenching tank, which is equivalent to cooling in the air. Due to the slow cooling speed, the decomposition of the supersaturated solid solution will reduce the aging strengthening effect, thereby reducing the mechanical properties and corrosion resistance of the product.
[0037] Principles and advantages
[0038] The present invention provides a high-strength rare earth modified aluminum alloy material and a preparation method thereof. The high-strength rare earth modified aluminum alloy material adopts a relatively high content of main alloying elements to improve the strength of the aluminum alloy material. In addition, rare earth elements are added on the basis of the national standard composition, and the rare earth elements are used to purify, refine, strengthen and other effects on the aluminum alloy, which conforms to the general action law of rare earth in aluminum alloy. The addition of rare earth makes the microstructure refinement one order of magnitude ahead of ordinary aluminum alloys, and precipitates a precipitated phase and a nano-scale strengthening phase with a stable structure, which is coherent or semi-coherent with the matrix, has a pinning effect on dislocations and subgrain boundaries, can effectively inhibit the growth of recrystallized grains, can significantly refine aluminum alloy grains, increase the recrystallization temperature of aluminum alloys, promote the precipitation of main strengthening phases, form a multi-level action mechanism such as a composite strengthening phase, achieve the effects of alloy solid solution strengthening, dispersion strengthening, precipitation strengthening, and fine grain strengthening, greatly improve the strength and plasticity of aluminum alloys, and effectively improve the comprehensive properties of aluminum alloys such as fatigue resistance and corrosion resistance.
[0039] During the preparation process, the present invention has formulated corresponding supporting smelting processes, including smelting, semi-continuous casting, ingot homogenization process, etc., so that it has a high-performance chemical basis, especially by adapting the homogenization treatment system and heat treatment system of the alloy composition of the present invention, so as to finally obtain a high-strength aluminum alloy with excellent mechanical properties, which meets the high-strength requirements of aluminum alloy materials for aerospace, rail transportation, and automotive lightweighting. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 Process flow chart of the present invention. DETAILED DESCRIPTION
[0041] The technical solution will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] A high-strength rare earth modified aluminum alloy material, whose chemical composition (by weight percentage) is: Mn (0.2-1.0%), Cu (1.0-1.5%), Zn (9.5-10.5%), Mg (2.0-3.0%), Zr (0.05-0.3%), Ti (0-0.3%), RE (0.05-0.4%), and the balance is Al and unavoidable impurities.
[0043] The high-strength rare earth modified aluminum alloy material has the following characteristics in the heat-treated state (T651 state): tensile strength Rm≥820MPa, yield strength Rp0.2≥800Mpa, and elongation after fracture A≥6%.
[0044] In the high-strength rare earth modified aluminum alloy material, the Si content in the aluminum alloy is less than 0.08%, the Fe content is less than 0.12%, the content of a single other element is less than 0.05%, and the combined content of other elements is less than 0.15%.
[0045] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0046] 1) In the dried metal and alloy raw materials, alloy elements Mn, Cu, Zr, and RE are added in the form of master alloys Al-Mn, Al-Cu, Al-Zr, and Al-RE, respectively, Ti is added to the alloy in the form of Al-Ti-C, and Zn and Mg are pure zinc ingots and pure magnesium ingots, so as to minimize the segregation of alloy elements in the ingots;
[0047] 2) Melting, semi-continuous casting, ingot homogenization, forward hot extrusion, and heat treatment are performed to obtain the above-mentioned aluminum alloy material.
[0048] Among them, the specific smelting and semi-continuous casting process for making high-strength rare earth modified aluminum alloy materials is as follows:
[0049] 3) Calculation of furnace charge ratio: a. Aluminum ingots, zinc ingots and magnesium ingots are added as pure metals, and alloy elements Mn, Cu, Zr and RE are added in the form of Al-10Mn, Al-20Cu, Al-4Zr and Al-10RE master alloys respectively to reduce the segregation of alloy elements in the ingot. The weight of the ingredients is recorded in the ingredient list and the number is recorded; c. The materials used are dried at 200℃ before use; d. The ingredients are calculated according to the mass percentage of the chemical composition.
[0050] 4) Weighing of alloy materials: a. Aluminum ingots are weighed with an electronic scale; b. Master alloys and alloying elements are weighed with an electronic balance. c. The allowable weight tolerance range is ±0.5%.
[0051] 5) When loading the furnace, first throw the broken aluminum and small materials to the bottom of the furnace to protect the bottom of the furnace. The temperature setting of the aluminum liquid: the aluminum liquid in the crucible furnace is set at 750℃, and the furnace gas temperature should be controlled at 850℃. After the aluminum liquid in the crucible reaches 700℃ and is completely melted, start to add Al-4Zr, Al-10Mn, Al-20Cu master alloys in turn and evenly, and then add Zn ingots, Al-10RE, Mg ingots, etc. It is strictly forbidden to expose the liquid surface or close to the bottom of the furnace. After all the furnace materials are melted, start stirring. When the temperature of the aluminum liquid is between 720 and 750℃, scrape off the scum on the surface. Safety measures: Gently put the master alloy material into the crucible. Excessive impact can easily cause the crucible to break; tools that contact the aluminum liquid must be fully dried before they are allowed to be used.
[0052] 6) Chemical composition analysis of samples: If the chemical composition is unqualified, adjust the method of adding elements according to the analysis results, and then degas and stir until it is qualified. Record the sample number: Use an oil pen to write the number on the ingredient list clearly and accurately on the sample.
[0053] 7) After the ingredients are qualified, transfer them to a static insulation furnace and stir them thoroughly. Use high-purity argon gas for refining, the refining time is 15 to 20 minutes, and the refining temperature is controlled at 730 to 740°C.
[0054] 8) The casting temperature is controlled at 690-710℃, Al-5Ti-0.2C wire is connected, double wire feeding is adopted, and the speed is 35-45mm / min. In actual operation, the filter plate adopts 30ppi+50ppi double-stage filtration during casting.
[0055] The relevant specific embodiments of the present invention are as follows:
[0056] Example 1
[0057] This embodiment provides a new type of high-strength rare earth modified aluminum alloy material, the chemical composition of which is shown in Table 1 below:
[0058] Table 1
[0059]
[0060] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0061] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, the temperature is uniformly raised to 405°C within 1.5 hours, then kept at this temperature for 6 hours, and then raised to 450°C again, kept at this temperature for 18 hours for homogenization treatment.
[0062] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 425℃, holding time: 80min; mold heating temperature: 430℃, holding time: 150min; extrusion rate: 1.0mm / s.
[0063] Heat treatment process: heat to 410℃ at a rate of 60℃ / h, keep warm for 1h, heat to 465℃ again, keep warm for 1.5h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 1.5%. Aging process: heat to 120℃, keep warm for 22h.
[0064] Example 2
[0065] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of the material is as shown in Example 1.
[0066] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0067] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 410°C within 2 hours, then keep warm for 7 hours, and then heat to 455°C again, keep warm for 20 hours for homogenization.
[0068] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 435℃, holding time: 90min; mold heating temperature: 450℃, holding time: 180min; extrusion rate: 1.2mm / s.
[0069] Heat treatment process: heat to 415℃ at a rate of 75℃ / h, keep warm for 1.5h, heat to 470℃ again, keep warm for 2h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 2.0%. Aging process: heat to 115℃, keep warm for 26h.
[0070] Example 3
[0071] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of the material is as shown in Example 1.
[0072] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0073] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 420°C within 2 hours, then keep warm for 8 hours, and then heat to 460°C again, keep warm for 19 hours for homogenization.
[0074] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 450℃, holding time: 100min; mold heating temperature: 460℃, holding time: 200min; extrusion rate: 2.0mm / s.
[0075] Heat treatment process: heat to 420℃ at a rate of 85℃ / h, keep warm for 1.5h, heat to 467℃ again, keep warm for 1.6h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rods are clamped on the stretching machine for stretching, and the stretching deformation is 2.5%. Aging process: heat to 125℃, keep warm for 24h.
[0076] Example 4
[0077] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is shown in Table 2 below:
[0078] Table 2
[0079]
[0080] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0081] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, the temperature is uniformly raised to 405°C within 1.5 hours, then kept at this temperature for 6 hours, and then raised to 450°C again, kept at this temperature for 18 hours for homogenization treatment.
[0082] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 425℃, holding time: 80min; mold heating temperature: 430℃, holding time: 150min; extrusion rate: 1.0mm / s.
[0083] Heat treatment process: heat to 410℃ at a rate of 60℃ / h, keep warm for 1h, heat to 465℃ again, keep warm for 1.5h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 1.5%. Aging process: heat to 120℃, keep warm for 22h.
[0084] Example 5
[0085] This embodiment provides a new type of high-strength rare earth modified aluminum alloy material, the chemical composition of which is as shown in Example 4.
[0086] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0087] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 410°C within 2 hours, then keep warm for 7 hours, and then heat to 455°C again, keep warm for 20 hours for homogenization.
[0088] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 435℃, holding time: 90min; mold heating temperature: 450℃, holding time: 180min; extrusion rate: 1.2mm / s.
[0089] Heat treatment process: heat to 415℃ at a rate of 75℃ / h, keep warm for 1.5h, heat to 470℃ again, keep warm for 2h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 2.0%. Aging process: heat to 115℃, keep warm for 26h.
[0090] Example 6
[0091] This embodiment provides a new type of high-strength rare earth modified aluminum alloy material, the chemical composition of which is as shown in Example 4.
[0092] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0093] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 420°C within 2 hours, then keep warm for 8 hours, and then heat to 460°C again, keep warm for 19 hours for homogenization.
[0094] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 450℃, holding time: 100min; mold heating temperature: 460℃, holding time: 200min; extrusion rate: 2.0mm / s.
[0095] Heat treatment process: heat to 420℃ at a rate of 85℃ / h, keep warm for 1.5h, heat to 467℃ again, keep warm for 1.6h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rods are clamped on the stretching machine for stretching, and the stretching deformation is 2.5%. Aging process: heat to 125℃, keep warm for 24h.
[0096] Example 7
[0097] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is shown in Table 3 below:
[0098] Table 3
[0099]
[0100]
[0101] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0102] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, the temperature is uniformly raised to 405°C within 1.5 hours, then kept at this temperature for 6 hours, and then raised to 450°C again, kept at this temperature for 18 hours for homogenization treatment.
[0103] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 425℃, holding time: 80min; mold heating temperature: 430℃, holding time: 150min; extrusion rate: 1.0mm / s.
[0104] Heat treatment process: heat to 410℃ at a rate of 60℃ / h, keep warm for 1h, heat to 465℃ again, keep warm for 1.5h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 1.5%. Aging process: heat to 120℃, keep warm for 22h.
[0105] Example 8
[0106] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of the material is as shown in Example 7.
[0107] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0108] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 410°C within 2 hours, then keep warm for 7 hours, and then heat to 455°C again, keep warm for 20 hours for homogenization.
[0109] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 435℃, holding time: 90min; mold heating temperature: 450℃, holding time: 180min; extrusion rate: 1.2mm / s.
[0110] Heat treatment process: heat to 415℃ at a rate of 75℃ / h, keep warm for 1.5h, heat to 470℃ again, keep warm for 2h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rod is clamped on the stretching machine for stretching, and the stretching deformation is 2.0%. Aging process: heat to 115℃, keep warm for 26h.
[0111] Example 9
[0112] This embodiment provides a high-strength rare earth modified aluminum alloy material, the chemical composition of the material is as shown in Example 7.
[0113] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0114] Homogenization process: To reduce the presence of compounds in the microstructure of the ingot after homogenization, uniformly heat to 420°C within 2 hours, then keep warm for 8 hours, and then heat to 460°C again, keep warm for 19 hours for homogenization.
[0115] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 450℃, holding time: 100min; mold heating temperature: 460℃, holding time: 200min; extrusion rate: 2.0mm / s.
[0116] Heat treatment process: heat to 420℃ at a rate of 85℃ / h, keep warm for 1.5h, heat to 467℃ again, keep warm for 1.6h. Take out and quickly transfer to 35℃ water, transfer time <10s. The dried extruded small rods are clamped on the stretching machine for stretching, and the stretching deformation is 2.5%. Aging process: heat to 125℃, keep warm for 24h.
[0117] Comparative Example 1
[0118] Comparative Example 1 provides a 7055 aluminum alloy material in the national standard GB / T3190-2020, and the chemical composition of the material is shown in Table 4 below:
[0119] Table 4
[0120]
[0121] The 7055 aluminum alloy material in the comparative example 1 is different from that in the example 1 only in composition, while other conditions such as the preparation method are the same as those in the example 1.
[0122] Comparative Example 2
[0123] Comparative Example 2 provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is the same as that of Experimental Example 1.
[0124] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material comprises the following steps:
[0125] The calculation of the furnace charge ratio, weighing of the alloy materials, furnace loading, and sampling and chemical composition analysis are the same as in Example 1.
[0126] The casting is semi-continuous casting, the casting temperature is 660°C, Al-5Ti-0.2C wire is connected, double wire feeding is adopted, 35-45mm / min.
[0127] During the casting process, the ingot had large shrinkage cavities and cracks due to the low casting temperature, and the casting was unsuccessful. Comparative Example 2 had no performance results.
[0128] Comparative Example 3
[0129] Comparative Example 3 provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is the same as that of Experimental Example 1.
[0130] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material is the same as that of Example 1 except that the homogenization process is different from that of Example 1.
[0131] The homogenization process is to uniformly heat the material to 450-460°C within 1.5-2 hours and then keep the temperature for 18 hours.
[0132] Comparative Example 4
[0133] Comparative Example 4 provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is the same as that of Experimental Example 1.
[0134] The preparation method of the above-mentioned novel high-strength rare earth modified aluminum alloy material is the same as that of Example 1 except that the forward extrusion process is different from that of Example 1.
[0135] Forward hot extrusion process: In the extrusion process, preheating temperature and time as well as extrusion speed are important processes. Ingot heating temperature: 465℃, holding time: 150min; mold heating temperature: 475℃, holding time: 210min; extrusion rate: 5mm / s.
[0136] Comparative Example 5
[0137] Comparative Example 5 provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is the same as that of Experimental Example 1.
[0138] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material is the same as that of Example 1 except that the positive heat treatment process is different from that of Example 1.
[0139] Heat treatment process: The heat treatment process is to heat up to 450℃ at a rate of 60℃ / h and keep it warm for 1.5-2h. Take it out and quickly transfer it to 35℃ water, and the transfer time is less than 10s. The extruded small rod after drying is clamped on the stretching machine and stretched, and the stretching deformation is 1.5%. Aging process: heat up to 110℃ and keep it warm for 22h.
[0140] Comparative Example 6
[0141] Comparative Example 6 provides a high-strength rare earth modified aluminum alloy material, the chemical composition of which is the same as that of Experimental Example 1.
[0142] The preparation method of the above-mentioned high-strength rare earth modified aluminum alloy material is the same as that of Example 1 except that the heat treatment process is different from that of Example 1.
[0143] Heat treatment process: heat to 410℃ at a rate of 60℃ / h, keep warm for 1h, then heat to 465℃ again, keep warm for 1.5h. Take out and quickly transfer to 35℃ water, transfer time <10s. Aging process: heat to 120℃, keep warm for 22h.
[0144] According to GB / T 228.1-2021, the performance of the aluminum alloy materials of Examples 1 to 9 and Comparative Examples 1 to 6 after heat treatment (T651) was tested, and the test results are shown in Table 5:
[0145] Table 5
[0146]
[0147] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that technicians in the relevant technical field can understand and use the present invention well. The present invention is only limited by the claims and their full scope and equivalents. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A high-strength rare earth modified aluminum alloy material, characterized in that: The chemical composition is as follows, by mass percentage: Mn 0.2-1.0%, Cu 1.0-1.5%, Zn 9.5-10.5%, Mg 2.0-3.0%, Zr0.05-0.3%, Ti 0-0.3%, RE 0.05-0.4%, and the balance is Al and unavoidable impurities.
2. The high-strength rare earth modified aluminum alloy material according to claim 1, characterized in that: The high-strength rare earth modified aluminum alloy material has the following chemical composition by mass percentage: Mn 0.3-0.8%, Cu 1.0-1.5%, Zn 9.5-10.5%, Mg 2.0-3.0%, Zr 0.05-0.3%, Ti 0.02-0.1%, RE 0.05-0.4%, and the balance is Al and unavoidable impurities.
3. A high-strength rare earth modified aluminum alloy material according to claim 1 or 2, characterized in that: The RE is selected from at least one of Sc, La, Ce, Y, Yb, and Er.
4. A high-strength rare earth modified aluminum alloy material according to claim 1 or 2, characterized in that: The high-strength rare earth modified aluminum alloy material has a tensile strength Rm≥820MPa, a yield strength Rp0.2≥800Mpa, and an elongation after fracture A≥6% under T651 heat treatment.
5. The method for preparing a high-strength rare earth modified aluminum alloy material according to any one of claims 1 to 4, characterized in that: The metal raw materials are mixed and smelted according to the designed proportion to obtain a melt, the melt is cast to obtain an ingot, the ingot is homogenized to obtain a homogenized billet, the homogenized billet is hot-extruded to obtain an extruded billet, and the extruded billet is heat-treated to obtain an aluminum alloy material.
6. The method for preparing a high-strength rare earth modified aluminum alloy material according to claim 5, characterized in that: The smelting process is as follows: firstly, crushed aluminum and recycled materials are thrown into the bottom of the furnace, and aluminum ingots are placed thereon to melt and obtain aluminum liquid, and then Al-20Cu, Al-4Zr, Al-10Mn, Al-10RE master alloy, Zn ingot and Mg ingot are uniformly added in sequence to obtain aluminum alloy liquid, and the aluminum alloy liquid is stirred, and when the temperature of the aluminum alloy liquid is 730-750°C, the slag is skimmed, and after the composition is qualified, argon gas is used for refining, and the refining temperature is 730-740°C, and the refining time is 15-20min.
7. The method for preparing a high-strength rare earth modified aluminum alloy material according to claim 6, characterized in that: The casting is semi-continuous casting, the casting temperature is controlled at 690-710° C., Al-5Ti-0.2C wire is connected, double wire feeding is adopted, and the speed is 35-45 mm / min.
8. The method for preparing a high-strength rare earth modified aluminum alloy material according to claim 6, characterized in that: The homogenization process is to uniformly heat the temperature to 400-420° C. within 1.5-2 hours, then keep the temperature for 5-8 hours, and then heat the temperature to 450-460° C. again, and keep the temperature for 18-20 hours.
9. The method for preparing a high-strength rare earth modified aluminum alloy material according to claim 6, characterized in that: The hot extrusion is forward hot extrusion. During the hot extrusion, the preheating temperature of the homogenized billet is 410-450° C., the preheating and heat preservation time of the homogenized billet is 75-120 min, the preheating temperature of the mold is 420-460° C., the preheating and heat preservation time of the mold is 120-240 min, and the extrusion rate is 0.5-4 mm / s.
10. The method for preparing a high-strength rare earth modified aluminum alloy material according to claim 6, characterized in that: The heat treatment process is to first subject the extruded billet to a solution treatment, then to a stretching deformation treatment, and then to an aging treatment; The process of the solution treatment is: firstly heating to 410-420°C at a rate of 50-100°C / h, keeping the temperature for 1-1.5h, then heating to 465-472°C again, keeping the temperature for 1.5-2h, then taking out the extruded billet and transferring it to water, controlling the transfer time to be less than 10s; The stretching deformation amount of the stretching deformation treatment is 1.5 to 3%; The temperature of the aging treatment is 115-125° C., and the time of the aging treatment is 20-26 hours.
Citation Information
Cited By
High-strength Al-Zn-Mg-Cu-Mn alloy suitable for friction stir additive manufacturing and forming process of high-strength Al-Zn-Mg-Cu-Mn alloy
CN121023325A
Preparation method of in-situ Y2O3 modified TA1 thin strip based on thin strip cast rolling
CN121911840A
A method for preparing in-situ Y2O3-modified TA1 thin strip based on thin strip casting and rolling
CN121911840B